MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Shell Carilon® DB6F1G30 Polyketone, Flame-Retarded, Tracking-Resistant, Glass-Reinforced Injection Molding Grade  (discontinued **)
Categories: Polymer; Thermoplastic; Polyketone; Polyketone, Glass Fiber Reinforced

Material Notes: Shell announced in Feb. 2000 that the Carilon product line is being discontinued. CARILON Polymer DB6F1G30 is a flame-retarded, 15 percent glass-fiber-reinforced, injection molding grade with mechanical properties which classify it as an engineering thermoplastic. This high modulus grade offers a UL94 V-1 rating, high comparative tracking and high glow-wire indices, all without the use of halogenated or red phosphorus flame retardants. The benign flame-retardant system used for CARILON Polymer DB6F1G30 ensures that the smoke density and toxicity are both low. Yet this grade retains the exceptional blend of properties of the base polymer, such as low moisture absorption, good toughness and high resistance to a wide range of chemicals. CARILON Polymer DB6F1G30 is easy to process on standard injection molding equipment. Cycle times are generally short and parts show good mold definition. CARILON Polymers' low moisture sensitivity means that no conditioning of parts before assembly or use is necessary.

Data provided by Shell Chemical.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.60 g/cc0.0578 lb/in³ASTM D792
Water Absorption 0.30 %0.30 %24 hour immersion; ASTM D570
Moisture Absorption at Equilibrium 0.45 %0.45 %at 50% RH; ASTM D570
Linear Mold Shrinkage, Flow 0.0030 cm/cm0.0030 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.011 cm/cm0.011 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 95.0 MPa13800 psiASTM D638
Elongation at Break 3.0 %3.0 %ASTM D638
Tensile Modulus 8.00 GPa1160 ksiASTM D638
Flexural Modulus 5.90 GPa856 ksiASTM D790
Izod Impact, Notched 1.17 J/cm2.19 ft-lb/inASTM D256
Charpy Impact Unnotched 4.00 J/cm²19.0 ft-lb/in²ISO 179
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmASTM D257
Surface Resistance 1.00e+13 ohm1.00e+13 ohmASTM D257
Dielectric Constant 6.2
@Frequency 1e+6 Hz
6.2
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 41.0 kV/mm
@Thickness 0.800 mm
1040 kV/in
@Thickness 0.0315 in
Short Term; ASTM D149
Dissipation Factor 0.030
@Frequency 1e+6 Hz
0.030
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 120 - 180 sec120 - 180 secUL-746A rating 5 (120-180 sec)
Comparative Tracking Index 450 V450 VUL746A
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °F
Deflection Temperature at 1.8 MPa (264 psi) 200 °C392 °FASTM D648
Flammability, UL94 V-1V-1
Oxygen Index 33 %33 %ISO 4589

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Shell Carilon® DB6G6P30 Polyketone, Lubricated, Glass-Reinforced, Injection Molding Grade
Shell Carilon® D26HM100 Polyketone, General-Purpose Injection Molding Grade
Shell Carilon® DP R1130 Polyketone, 30% Glass Fiber Reinforced
Shell Carilon® DP P1000 Polyketone
Shell Carilon® DB6G6A10 Polyketone, 30% Glass-Reinforced General-Purpose Injection Molding Grade

PCAR11 / 27920

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.