MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polyethylene Terephthalate (PET), Glass Fiber Filled, Flame Retardant
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), Glass Fiber Filled, Flame Retardant

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyethylene Terephthalate (PET), Glass Fiber Filled, Flame Retardant". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.49 - 1.80 g/cc0.0538 - 0.0650 lb/in³Average value: 1.63 g/cc Grade Count:59
Filler Content 15.0 - 33.0 %15.0 - 33.0 %Average value: 23.8 % Grade Count:18
Water Absorption 0.0500 - 0.750 %0.0500 - 0.750 %Average value: 0.164 % Grade Count:29
Moisture Absorption at Equilibrium 0.150 %0.150 %Average value: 0.150 % Grade Count:3
Maximum Moisture Content 0.02000.0200Average value: 0.0200 Grade Count:3
Linear Mold Shrinkage 0.000 - 0.0110 cm/cm0.000 - 0.0110 in/inAverage value: 0.00352 cm/cm Grade Count:51
Linear Mold Shrinkage, Transverse 0.00200 - 0.0115 cm/cm0.00200 - 0.0115 in/inAverage value: 0.00760 cm/cm Grade Count:26
Melt Flow 6.00 - 45.0 g/10 min6.00 - 45.0 g/10 minAverage value: 22.7 g/10 min Grade Count:3
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 88.0 - 95.088.0 - 95.0Average value: 93.0 Grade Count:8
Hardness, Rockwell R 111 - 120111 - 120Average value: 118 Grade Count:13
Tensile Strength, Ultimate 78.6 - 172 MPa11400 - 24900 psiAverage value: 124 MPa Grade Count:51
 50.0 - 170 MPa
@Temperature -40.0 - 120 °C
7250 - 24700 psi
@Temperature -40.0 - 248 °F
Average value: 101 MPa Grade Count:2
Tensile Strength, Yield 108 - 157 MPa15700 - 22800 psiAverage value: 133 MPa Grade Count:7
Elongation at Break 0.500 - 6.00 %0.500 - 6.00 %Average value: 2.27 % Grade Count:57
 1.70 - 5.70 %
@Temperature -40.0 - 120 °C
1.70 - 5.70 %
@Temperature -40.0 - 248 °F
Average value: 3.92 % Grade Count:2
Modulus of Elasticity 6.00 - 14.6 GPa870 - 2120 ksiAverage value: 10.4 GPa Grade Count:23
 3.013 - 12.5 GPa
@Temperature -40.0 - 150 °C
437.0 - 1810 ksi
@Temperature -40.0 - 302 °F
Average value: 6.79 GPa Grade Count:2
Flexural Yield Strength 120 - 278 MPa17400 - 40300 psiAverage value: 185 MPa Grade Count:50
 85.0 - 275 MPa
@Temperature -40.0 - 120 °C
12300 - 39900 psi
@Temperature -40.0 - 248 °F
Average value: 180 MPa Grade Count:1
Flexural Modulus 5.52 - 16.0 GPa800 - 2320 ksiAverage value: 9.35 GPa Grade Count:57
 2.97 - 2.97 GPa
@Temperature 120 - 120 °C
431 - 431 ksi
@Temperature 248 - 248 °F
Average value: 2.97 GPa Grade Count:1
Compressive Yield Strength 98.0 - 200 MPa14200 - 29000 psiAverage value: 131 MPa Grade Count:7
Poissons Ratio 0.330 - 0.3500.330 - 0.350Average value: 0.337 Grade Count:6
Shear Modulus 0.525 - 2.432 GPa
@Temperature -50.0 - 160 °C
76.1 - 352.7 ksi
@Temperature -58.0 - 320 °F
Average value: 1.39 GPa Grade Count:1
Secant Modulus  4.65654 - 8.95349 GPa
@Temperature -20.0 - 40.0 °C
675.385 - 1298.61 ksi
@Temperature -4.00 - 104 °F
Average value: 7.36 GPa Grade Count:1
 4.65654 - 8.95349 GPa
@Strain 0.520 - 2.83 %
675.385 - 1298.61 ksi
@Strain 0.520 - 2.83 %
Average value: 7.36 GPa Grade Count:1
Izod Impact, Notched 0.530 - 1.60 J/cm0.993 - 3.00 ft-lb/inAverage value: 0.834 J/cm Grade Count:39
 0.500 - 0.800 J/cm
@Temperature -40.0 - -20.0 °C
0.937 - 1.50 ft-lb/in
@Temperature -40.0 - -4.00 °F
Average value: 0.656 J/cm Grade Count:5
Izod Impact, Unnotched 0.834 - 8.70 J/cm1.56 - 16.3 ft-lb/inAverage value: 3.24 J/cm Grade Count:6
Izod Impact, Notched (ISO) 11.5 - 11.5 kJ/m²
@Temperature -40.0 - -40.0 °C
5.47 - 5.47 ft-lb/in²
@Temperature -40.0 - -40.0 °F
Average value: 11.5 kJ/m² Grade Count:1
Charpy Impact Unnotched 3.00 - 4.60 J/cm²14.3 - 21.9 ft-lb/in²Average value: 3.84 J/cm² Grade Count:12
 2.00 - 4.00 J/cm²
@Temperature -40.0 - -30.0 °C
9.52 - 19.0 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 3.07 J/cm² Grade Count:6
Charpy Impact, Notched 0.550 - 1.15 J/cm²2.62 - 5.47 ft-lb/in²Average value: 0.831 J/cm² Grade Count:21
 0.600 - 1.40 J/cm²
@Temperature -40.0 - -30.0 °C
2.86 - 6.66 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 0.880 J/cm² Grade Count:9
Taber Abrasion, mg/1000 Cycles 25.0 - 36.025.0 - 36.0Average value: 30.6 Grade Count:5
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+13 - 1.00e+18 ohm-cm1.00e+13 - 1.00e+18 ohm-cmAverage value: 3.34e+16 ohm-cm Grade Count:40
Surface Resistance 1.00e+13 - 1.00e+15 ohm1.00e+13 - 1.00e+15 ohmAverage value: 4.42e+14 ohm Grade Count:10
Dielectric Constant 3.50 - 4.803.50 - 4.80Average value: 3.93 Grade Count:14
Dielectric Strength 18.0 - 40.0 kV/mm457 - 1020 kV/inAverage value: 27.2 kV/mm Grade Count:29
Dissipation Factor 0.00700 - 0.03090.00700 - 0.0309Average value: 0.0153 Grade Count:11
Arc Resistance 80.0 - 85.0 sec80.0 - 85.0 secAverage value: 82.3 sec Grade Count:7
Comparative Tracking Index 15.0 - 600 V15.0 - 600 VAverage value: 247 V Grade Count:29
 
Thermal PropertiesMetricEnglishComments
CTE, linear 14.0 - 33.0 µm/m-°C7.78 - 18.3 µin/in-°FAverage value: 22.8 µm/m-°C Grade Count:18
 11.0 - 19.0 µm/m-°C
@Temperature 55.0 - 160 °C
6.11 - 10.6 µin/in-°F
@Temperature 131 - 320 °F
Average value: 14.2 µm/m-°C Grade Count:5
CTE, linear, Transverse to Flow 51.0 - 96.0 µm/m-°C28.3 - 53.3 µin/in-°FAverage value: 76.8 µm/m-°C Grade Count:8
 81.0 - 125 µm/m-°C
@Temperature 55.0 - 160 °C
45.0 - 69.4 µin/in-°F
@Temperature 131 - 320 °F
Average value: 106 µm/m-°C Grade Count:5
Specific Heat Capacity 1.72 - 1.72 J/g-°C
@Temperature 280 - 280 °C
0.411 - 0.411 BTU/lb-°F
@Temperature 536 - 536 °F
Average value: 1.72 J/g-°C Grade Count:1
Thermal Conductivity 0.240 - 0.240 W/m-K
@Temperature 280 - 280 °C
1.67 - 1.67 BTU-in/hr-ft²-°F
@Temperature 536 - 536 °F
Average value: 0.240 W/m-K Grade Count:1
Melting Point 245 - 255 °C473 - 491 °FAverage value: 251 °C Grade Count:27
Maximum Service Temperature, Air 140 - 220 °C284 - 428 °FAverage value: 162 °C Grade Count:8
Hot Ball Pressure Test 230 - 245 °C446 - 473 °FAverage value: 241 °C Grade Count:9
Deflection Temperature at 0.46 MPa (66 psi) 230 - 250 °C446 - 482 °FAverage value: 241 °C Grade Count:29
Deflection Temperature at 1.8 MPa (264 psi) 195 - 243 °C383 - 469 °FAverage value: 220 °C Grade Count:52
Vicat Softening Point 210 - 246 °C410 - 475 °FAverage value: 231 °C Grade Count:9
Glass Transition Temp, Tg 90.0 °C194 °FAverage value: 90.0 °C Grade Count:6
UL RTI, Electrical 130 - 155 °C266 - 311 °FAverage value: 150 °C Grade Count:11
Flammability, UL94 V-2 - 5VAV-2 - 5VAGrade Count:55
Oxygen Index 32.0 - 36.0 %32.0 - 36.0 %Average value: 33.1 % Grade Count:11
Glow Wire Test 775 - 960 °C1430 - 1760 °FAverage value: 873 °C Grade Count:11
 
Processing PropertiesMetricEnglishComments
Processing Temperature 243 - 293 °C470 - 560 °FAverage value: 271 °C Grade Count:6
Nozzle Temperature 271 - 295 °C520 - 563 °FAverage value: 284 °C Grade Count:4
Melt Temperature 230 - 300 °C446 - 572 °FAverage value: 271 °C Grade Count:23
Mold Temperature 40.0 - 163 °C104 - 325 °FAverage value: 106 °C Grade Count:28
Drying Temperature 110 - 150 °C230 - 302 °FAverage value: 125 °C Grade Count:21
Moisture Content 0.0100 - 0.0200 %0.0100 - 0.0200 %Average value: 0.0175 % Grade Count:8
Injection Pressure 3.50 - 120 MPa508 - 17400 psiAverage value: 66.8 MPa Grade Count:5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyethylene Terephthalate (PET), Unreinforced
Overview of materials for Polyethylene Terephthalate (PET), Unreinforced, Flame Retardant
Overview of materials for Polyethylene Terephthalate (PET), 20% Glass Reinforced
Overview of materials for Polyethylene Terephthalate (PET), 50% Glass Reinforced
Overview of materials for Polyethylene Terephthalate (PET), 30% Glass Reinforced

O3310 / 78196

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.