MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Titanium Ti-11.5Mo-6Zr-4.5Sn, ST 720°C, Aged 495°C
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Microstructure: Beta alloy, can be aged without forming intermetallic compounds.

Characteristics: High strength, good hardenability, good resistance to stress corrosion, good cold-formability.

Applications: Aircraft fasteners and sheet metal parts, to a lesser extent - plate and forging applications.

5 other heat treatments of this alloy are in MatWeb.

Key Words: Ti Beta III; UNS R58030
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 5.06 g/cc0.183 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 369369Estimated from Rockwell C.
Hardness, Knoop 403403Estimated from Rockwell C.
Hardness, Rockwell C 4040
Hardness, Vickers 386386Estimated from Rockwell C.
Tensile Strength >= 1070 MPa
@Temperature 371 °C
>= 155000 psi
@Temperature 700 °F
Tensile Strength, Ultimate 1240 MPa180000 psi
Tensile Strength, Yield 1200 MPa174000 psi
Elongation at Break 6.0 %6.0 %
Reduction of Area 10 %10 %
Creep Strength 689 MPa
@Temperature 371 °C,
Time >=3.60e+6 sec
99900 psi
@Temperature 700 °F,
Time >=1000 hour
strain 0.4%
Rupture Strength 1030 MPa
@Temperature 371 °C,
Time 3.60e+6 sec
149000 psi
@Temperature 700 °F,
Time 1000 hour
Modulus of Elasticity 108 GPa15700 ksi
Modulus of Rigidity 40.7 GPa5900 ksi
Compressive Yield Strength 1280 MPa186000 psi
Compressive Modulus 110 GPa16000 ksi
Notched Tensile Strength 1520 MPa220000 psiKt (stress concentration factor) = 6.1
Poissons Ratio 0.310.31
Fatigue Strength  380 MPa
@# of Cycles 1.00e+7
55100 psi
@# of Cycles 1.00e+7
Kt (stress concentration factor) = 3.0
 590 MPa
@# of Cycles 1.00e+7
85600 psi
@# of Cycles 1.00e+7
 1000 MPa
@# of Cycles 1.00e+6
145000 psi
@# of Cycles 1.00e+6
Fracture Toughness 60.0 MPa-m½54.6 ksi-in½K(IC)
Shear Modulus 41.0 GPa5950 ksi
Shear Strength 720 MPa104000 psiUltimate shear strength
Charpy Impact 8.13 J6.00 ft-lb
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000156 ohm-cm0.000156 ohm-cm
Magnetic Permeability 1.01.0
 
Thermal PropertiesMetricEnglishComments
CTE, linear  7.60 µm/m-°C
@Temperature 20.0 - 100 °C
4.22 µin/in-°F
@Temperature 68.0 - 212 °F
 8.10 µm/m-°C
@Temperature 20.0 - 315 °C
4.50 µin/in-°F
@Temperature 68.0 - 599 °F
average
 8.70 µm/m-°C
@Temperature 20.0 - 540 °C
4.83 µin/in-°F
@Temperature 68.0 - 1000 °F
average
Specific Heat Capacity 0.525 J/g-°C0.125 BTU/lb-°FTypical value for titanium alloys.
Thermal Conductivity 6.28 W/m-K43.6 BTU-in/hr-ft²-°F
Melting Point 1573 - 1690 °C2863 - 3070 °F
Solidus 1573 °C2863 °F
Liquidus 1690 °C3070 °F
Beta Transus 760 °C1400 °FSlow transition kinetics
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
 <= 0.10 %<= 0.10 %
Hydrogen, H <= 0.020 %<= 0.020 %
 <= 0.020 %<= 0.020 %
Iron, Fe <= 0.35 %<= 0.35 %
 <= 0.35 %<= 0.35 %
Nitrogen, N <= 0.050 %<= 0.050 %
 <= 0.050 %<= 0.050 %
Other, each <= 0.010 %<= 0.010 %
 <= 0.050 %<= 0.050 %
Other, total <= 0.040 %<= 0.040 %
 <= 0.30 %<= 0.30 %
Oxygen, O <= 0.18 %<= 0.18 %
 <= 0.18 %<= 0.18 %
Tin, Sn 3.75 - 5.25 %3.75 - 5.25 %
Titanium, Ti 86.27 - 91.75 %86.27 - 91.75 %As Balance; Elemental Composition per ASTM B265
Zirconium, Zr 4.5 - 7.5 %4.5 - 7.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-13V-11Cr-3Al; (Ti-13-11-3) Annealed 850°C (1560°F) + Aged 510°C 8 hr
Titanium Ti-13V-11Cr-3Al (Ti-13-11-3) Aged 490°C
Titanium Ti-13V-11Cr-3Al (Ti-13-11-3) Aged 400°C
Titanium Ti-13V-11Cr-3Al (Ti-13-11-3) SolnTreat; Age 450°C
Titanium Ti-13V-11Cr-3Al (Ti-13-11-3) Solution Treated

MTB031 / 14153

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.