MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Rynite® FR515 NC010 PET-GF15FR(17)
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), Glass Fiber Filled, Flame Retardant

Material Notes: 15% Glass Reinforced, Flame Retardant, Polyethylene Terephthalate

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.53 g/cc0.0553 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0030 cm/cm0.0030 in/inISO 294-4, 2577
 0.0050 cm/cm0.0050 in/inannealed; ISO 294-4
 0.0010 cm/cm
@Treatment Temp. 80.0 °C,
Time 173000 sec
0.0010 in/in
@Treatment Temp. 176 °F,
Time 48.0 hour
Postmolding shrinkage; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/inISO 294-4, 2577
 0.0115 cm/cm0.0115 in/inannealed; ISO 294-4
 0.0025 cm/cm
@Treatment Temp. 80.0 °C,
Time 173000 sec
0.0025 in/in
@Treatment Temp. 176 °F,
Time 48.0 hour
Postmolding shrinkage; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 8888ISO 2039-2
Hardness, Rockwell R 120120ISO 2039-2
Tensile Strength at Break 107 MPa15500 psiISO 527-1/-2
Elongation at Break 2.6 %2.6 %ISO 527-1/-2
Tensile Modulus 6.80 GPa986 ksiISO 527-1/-2
Flexural Strength 170 MPa24700 psiISO 178
Flexural Modulus 5.94 GPa862 ksiISO 178
Compressive Strength 170 MPa24700 psiISO 604
Poissons Ratio 0.350.35
Shear Strength 50.0 MPa7250 psiASTM D 732
Charpy Impact Unnotched  2.00 J/cm²
@Temperature -40.0 °C
9.52 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eU
 3.50 J/cm²
@Temperature -30.0 °C
16.7 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 4.00 J/cm²
@Temperature 23.0 °C
19.0 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.700 J/cm²
@Temperature -40.0 °C
3.33 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eA
 0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.800 J/cm²
@Temperature 23.0 °C
3.81 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 62631-3-2
Dielectric Constant  3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 62631-2-1
 3.8
@Frequency 100 Hz
3.8
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 34.0 kV/mm864 kV/inIEC 60243-1
Dissipation Factor  0.0090
@Frequency 100 Hz
0.0090
@Frequency 100 Hz
IEC 62631-2-1
 0.015
@Frequency 1e+6 Hz
0.015
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 175 - 249 V175 - 249 VPLC 3; UL 746A
 225 V225 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 18.0 µm/m-°C10.0 µin/in-°FISO 11359-1/-2
 12.0 µm/m-°C
@Temperature 55.0 - 160 °C
6.67 µin/in-°F
@Temperature 131 - 320 °F
ISO 11359-1/-2
 33.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
18.3 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 88.0 µm/m-°C48.9 µin/in-°FISO 11359-1/-2
 70.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
 105 µm/m-°C
@Temperature 55.0 - 160 °C
58.3 µin/in-°F
@Temperature 131 - 320 °F
ISO 11359-1/-2
Thermal Conductivity 0.250 W/m-K1.74 BTU-in/hr-ft²-°FSolid
Melting Point 254 °C489 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 240 °C464 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 200 °C392 °FISO 75-1/-2
Vicat Softening Point 210 °C410 °F50°C/h, 50N; ISO 306
Glass Transition Temp, Tg 90.0 °C194 °F10°C/min; ISO 11357-1/-2
Flammability, UL94  V-0
@Thickness 0.860 mm
V-0
@Thickness 0.0339 in
IEC 60695-11-10
 5VA
@Thickness 1.50 mm
5VA
@Thickness 0.0591 in
IEC 60695-11-20
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
DNI; ISO 3795 (FMVSS 302)
Oxygen Index 32 %32 %ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 °C536 °FOptimum, Injection
 270 - 290 °C518 - 554 °FRange, Injection
Mold Temperature 110 °C230 °FOptimum, Injection
 100 - 120 °C212 - 248 °FInjection
Ejection Temperature 170 °C338 °FInjection
Drying Temperature 120 °C248 °FInjection
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.020 %<= 0.020 %Injection
Hold Pressure >= 80.0 MPa>= 11600 psiInjection
 
Descriptive Properties
AdditivesFlame retardant
 Release agent
Back pressureAs low as possible
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
Max. screw tangential speed (m/s)0.2Injection
Part Marking Code>PET-GF15FR(17)<ISO 11469
PolymerPET-GF15 FR
Processing Hold Pressure Time (s/mm)4Injection
Resin IdentificationPET-GF15FR(17)ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Crastin® S650FR NC010 PBT-FR(17)
Celanese Crastin® SK601 NC010 PBT-GF10
Celanese Rynite® 530 NC010 PET-GF30
Celanese Rynite® FR530 NC010 PET-GF30FR(17)
Celanese Crastin® S600F40 NC010 PBT

PDSX5271 / 197911

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.