MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger TECATEC PEI GW50 PL V02 natural - Polyetherimide, Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyetherimide (PEI); Polyetherimide (PEI), 10% Glass Fiber

Material Notes:
  • electrically insulating
  • inherent flame resistance
  • very good mechanical strength
Target Industries:
  • automotive industry
  • mechanical engineering
  • oil and gas industry
  • safety engineering
  • sporting goods

Information provided by Ensinger Inc.

Vendors: Ensinger TECAPEI™ glass fiber reinforced shapes, made from ULTEM® PEI with Ensinger's proprietary extrusion techniques, provide superior tensile strength, rigidity, and dimensional stability for your most demanding PEI applications.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.90 g/cc0.0686 lb/in³
Filler Content 50 %50 %Fiber volume
 50.0 %50.0 %Fiber Volume
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 450 MPa65300 psiISO 527-4
Modulus of Elasticity 24.0 GPa3480 ksiISO 527-4
Flexural Strength 570 MPa82700 psiISO 14125
Flexural Modulus 26.0 GPa3770 ksiISO 14125
Compressive Strength 670 MPa97200 psiISO 14126
Compressive Modulus 27.0 GPa3920 ksiISO 14126
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 10.0 µm/m-°C5.56 µin/in-°F
CTE, linear, Transverse to Flow 10.0 µm/m-°C5.56 µin/in-°F
Maximum Service Temperature, Air 180 °C356 °Flong term
 200 °C392 °Fshort term
Glass Transition Temp, Tg 217 °C423 °F
 
Processing PropertiesMetricEnglishComments
Drying Temperature 150 °C302 °F
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hour
 
Descriptive Properties
Colornatural
General material information0-90°Fiber orientation
 1-95 mmthickness
 280 g/m²Fiber areal weight
 422 g/m²Areal weight finished product
 625x525 mmMaterial widths
 E glassFiber type
 US 7781Fiber architecture
Resin weight content (%)33.7

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PENSIN8230 / 319158

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.