System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Addiplast Addinyl C2 V40 Nylon 66/6, 40% Glass Filled
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6/66
;
Nylon 66/6, 40% Glass Fiber Reinforced
Material Notes:
Glass fiber reinforced, high strength
Information provided by Addiplast.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.46
g/cc
0.0527
lb/in³
ISO 1183/A
Mechanical Properties
Metric
English
Comments
Hardness, Shore D
79
79
Conditioned; ISO 868
85
85
ISO 868
Tensile Strength at Break
130
MPa
18900
psi
Conditioned; ISO R 527
195
MPa
28300
psi
ISO R 527
Elongation at Yield
3.0 %
3.0 %
ISO R 527
6.0 %
6.0 %
Conditioned; ISO R 527
Modulus of Elasticity
6.10
GPa
885
ksi
Conditioned; ISO 178
11.5
GPa
1670
ksi
ISO 178
Izod Impact, Notched (ISO)
16.0
kJ/m²
7.61
ft-lb/in²
ISO 180/1A
22.0
kJ/m²
10.5
ft-lb/in²
Conditioned; ISO 180/1A
Charpy Impact Unnotched
6.50
J/cm²
30.9
ft-lb/in²
ISO 179/IeU
7.50
J/cm²
35.7
ft-lb/in²
Conditioned; ISO 179/IeU
Charpy Impact, Notched
1.10
J/cm²
5.23
ft-lb/in²
ISO 179/IeA
1.80
J/cm²
8.57
ft-lb/in²
Conditioned; ISO 179/IeA
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+12
ohm-cm
1.00e+12
ohm-cm
Conditioned; CEI 60093
1.00e+15
ohm-cm
1.00e+15
ohm-cm
CEI 60093
Dielectric Strength
30.0
kV/mm
762
kV/in
Conditioned; CEI 60243-1
35.0
kV/mm
889
kV/in
CEI 60243-1
Comparative Tracking Index
550
V
550
V
CEI 60112/Solution A
Thermal Properties
Metric
English
Comments
CTE, linear
30.0
µm/m-°C
16.7
µin/in-°F
ASTM E831
Melting Point
243
°C
469
°F
ISO 3146/C2
Deflection Temperature at 1.8 MPa (264 psi)
235
°C
455
°F
ISO 75-2/AF
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Celanese Zytel® HTN52G45HSL BK083 PA6T/66-GF45
Celanese Zytel® HTN52G35HSL BK083 PA6T/66-GF35
Celanese Nilit FRIANYL C73 GV40 Nylon 6.6/6 for injection molding, 40% glass fiber reinforced
Celanese Celstran® PA66-GF40-0101P10/11 PA666, 40% Glass Reinforced
Akro-Plastic Akromid® C3 GF 40 1 (4658) PA66/6 Dry, 40% Glass Filled
PFADD891 / 156105
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.