MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Bada BADAMID® B70 FR HF H UV natural Nylon 6, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced, Flame Retardant

Material Notes: Non-halogen and phosphorus-free flame-resistant injection molding grade with medium viscosity, heat- and UV-stabilized

Information provided by Bada

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.18 g/cc0.0426 lb/in³ISO 1183
Moisture Absorption 2.50 %2.50 %50% r.h.; ISO 62
Water Absorption at Saturation 8.1 %8.1 %ISO 62
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 75.0 MPa10900 psi5 mm/min; ISO 527-1/2
Elongation at Break 14 %14 %5 mm/min; ISO 527-1/2
Tensile Modulus 3.70 GPa537 ksi1 mm/min; ISO 527-1/2
Izod Impact, Notched (ISO)  3.00 kJ/m²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
ISO 180/1A
 5.00 kJ/m²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Charpy Impact Unnotched NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.300 J/cm²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC-62631-3-1
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC-62631-3-2
Dielectric Constant 3.7
@Frequency 1e+6 Hz
3.7
@Frequency 1e+6 Hz
IEC-62631-2-1
Comparative Tracking Index 500 V500 VIEC-60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 222 °C432 °F10 K/min; ISO 3146
Maximum Service Temperature, Air 185 °C365 °Fsome hours; EC-60216
 85.0 °C
@Time 7.20e+7 sec
185 °F
@Time 20000 hour
EC-60216
Deflection Temperature at 0.46 MPa (66 psi) 190 °C374 °FISO 75-1/2
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C176 °FISO 75-1/2
Flammability, UL94 V-2
@Thickness 1.60 mm
V-2
@Thickness 0.0630 in
Glow Wire Flammability Index 960 °C
@Thickness 1.60 mm
1760 °F
@Thickness 0.0630 in
IEC-60695-2-12
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 - 280 °C482 - 536 °F
Mold Temperature 80.0 - 90.0 °C176 - 194 °F
Drying Temperature 80.0 °C176 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Moisture Content <= 0.15 %<= 0.15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBADA132 / 286965

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.