MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Mocom (ALBIS) ALTECH® PA66 A 1000/517.01 IM Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Unreinforced

Material Notes: Base Polymer: Polyamide 66

Special Features: Heat ageing stabilization, easy release (demolding), high flow, modified bonding properties to PVC

Typical Application: Various

Information provided by Albis Plastics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.13 g/cc0.0408 lb/in³ISO 1183
Maximum Moisture Content 0.150.15
Linear Mold Shrinkage, Flow 0.027 - 0.031 cm/cm
@Time 86400 sec
0.027 - 0.031 in/in
@Time 24.0 hour
ISO 294-4
Linear Mold Shrinkage, Transverse 0.018 - 0.022 cm/cm
@Time 86400 sec
0.018 - 0.022 in/in
@Time 24.0 hour
ISO 294-4
Melt Flow 6.0 g/10 min
@Load 5.00 kg,
Temperature 275 °C
6.0 g/10 min
@Load 11.0 lb,
Temperature 527 °F
ISO 1133
Storage Temperature <= 30.0 °C<= 86.0 °Fdry, protected from light
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 65.0 MPa9430 psiISO 527
Elongation at Break 30 %30 %ISO 527
Elongation at Yield 5.0 %5.0 %ISO 527
Tensile Modulus 2.50 GPa363 ksiISO 527
Flexural Strength 95.0 MPa13800 psiISO 178
Flexural Modulus 2.45 GPa355 ksiISO 178
Charpy Impact Unnotched  10.0 J/cm²
@Temperature -40.0 °C
47.6 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.700 J/cm²
@Temperature -40.0 °C
3.33 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eA
 1.50 J/cm²
@Temperature 23.0 °C
7.14 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 262 °C504 °FISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C158 °FISO 75-1/-2
Vicat Softening Point 220 °C428 °FB50; ISO 306
 
Processing PropertiesMetricEnglishComments
Melt Temperature 270 - 290 °C518 - 554 °FInjection molding
Mold Temperature 40.0 - 80.0 °C104 - 176 °FInjection molding
Drying Temperature 80.0 °C
@Time 7200 - 43200 sec
176 °F
@Time 2.00 - 12.0 hour
in a dry air (desiccant) dryer
 
Descriptive Properties
Base PolymerPolyamide 66

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Toagosei America Aron Alpha® Industrial Krazy Glue™ 101 Cyanoacrylate Adhesive
Taiwan Sheen Soon Sheenthane® AH-701 TPU for Hotmelt Adhesive
SunChemical Gwent C2010517D4 Carbon/Graphite Ink
Parson Adhesives PARTITE® 7300 Methacrylate Structural Adhesive
Nylene® Nylene NX4795 Nylon 6

PALBIS8719 / 242778

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.