Physical Properties | Metric | English | Comments |
---|
Density | 1.20 - 1.67 g/cc | 0.0434 - 0.0603 lb/in³ |
| 1.136 - 1.20 g/cc @Temperature 220 - 270 °C | 0.04104 - 0.0434 lb/in³ @Temperature 428 - 518 °F |
Filler Content | 25.0 - 33.0 % | 25.0 - 33.0 % |
Water Absorption | 0.130 - 9.00 % | 0.130 - 9.00 % |
Moisture Absorption at Equilibrium | 0.170 - 7.10 % | 0.170 - 7.10 % |
| 0.700 - 2.50 % @Temperature 70.0 - 70.0 °C | 0.700 - 2.50 % @Temperature 158 - 158 °F |
| 0.550 - 1.55 % @Temperature 70.0 - 70.0 °C | 0.550 - 1.55 % @Temperature 158 - 158 °F |
| 0.550 - 1.55 % @Time 180000 - 1.44e+6 sec | 0.550 - 1.55 % @Time 50.0 - 400 hour |
Water Absorption at Saturation | 1.00 - 8.20 % | 1.00 - 8.20 % |
Additive Loading | 30.0 - 33.0 % | 30.0 - 33.0 % |
Viscosity | 2.60 - 50.0 cP | 2.60 - 50.0 cP |
| 30.0 - 500 cP @Temperature 230 - 270 °C | 30.0 - 500 cP @Temperature 446 - 518 °F |
| 30.0 - 500 cP @Shear Rate 100 - 10000 1/s | 30.0 - 500 cP @Shear Rate 100 - 10000 1/s |
Viscosity Test | 125 - 150 cm³/g | 1.25 - 1.50 dl/g |
Viscosity Number | 125 - 230 cm³/g | 1.25 - 2.30 dl/g |
Maximum Moisture Content | 0.0200 - 0.200 | 0.0200 - 0.200 |
Linear Mold Shrinkage | 0.000500 - 0.0650 cm/cm | 0.000500 - 0.0650 in/in |
| 0.00100 - 0.00300 cm/cm @Temperature 80.0 - 80.0 °C | 0.00100 - 0.00300 in/in @Temperature 176 - 176 °F |
Linear Mold Shrinkage, Transverse | 0.00100 - 0.0650 cm/cm | 0.00100 - 0.0650 in/in |
| 0.00500 - 0.00700 cm/cm @Temperature 80.0 - 80.0 °C | 0.00500 - 0.00700 in/in @Temperature 176 - 176 °F |
Melt Flow | 1.00 - 101 g/10 min | 1.00 - 101 g/10 min |
Spiral Flow | 50.0 - 715 cm | 19.7 - 281 in |
Ash | 25.0 - 37.0 % | 25.0 - 37.0 % |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell L | 102 - 115 | 102 - 115 |
Hardness, Rockwell M | 80.0 - 121 | 80.0 - 121 |
Hardness, Rockwell R | 82.0 - 122 | 82.0 - 122 |
| 12.0 - 12.0 @Temperature 80.0 - 80.0 °C | 12.0 - 12.0 @Temperature 176 - 176 °F |
Hardness, Shore D | 76.0 - 89.0 | 76.0 - 89.0 |
Hardness, Shore M | 100 | 100 |
Ball Indentation Hardness | 70.0 - 280 MPa | 10200 - 40600 psi |
Tensile Strength, Ultimate | 12.2 - 1500 MPa | 1770 - 218000 psi |
| 20.0 - 283 MPa @Temperature -40.0 - 150 °C | 2900 - 41000 psi @Temperature -40.0 - 302 °F |
| 125 - 150 MPa @Temperature 70.0 - 70.0 °C | 18100 - 21800 psi @Temperature 158 - 158 °F |
| 125 - 150 MPa @Time 180000 - 1.44e+6 sec | 18100 - 21800 psi @Time 50.0 - 400 hour |
| 30.0 - 170 MPa @Strain 1.00 - 2.00 % | 4350 - 24700 psi @Strain 1.00 - 2.00 % |
| 30.0 - 170 MPa @Temperature -20.0 - 150 °C | 4350 - 24700 psi @Temperature -4.00 - 302 °F |
Tensile Strength, Yield | 3.00 - 193 MPa | 435 - 28000 psi |
| 111 - 214 MPa @Temperature -40.0 - 80.0 °C | 16100 - 31000 psi @Temperature -40.0 - 176 °F |
Elongation at Break | 0.800 - 180 % | 0.800 - 180 % |
| 2.40 - 12.0 % @Temperature -40.0 - 150 °C | 2.40 - 12.0 % @Temperature -40.0 - 302 °F |
Elongation at Yield | 1.50 - 14.0 % | 1.50 - 14.0 % |
| 4.60 - 7.60 % @Temperature 60.0 - 150 °C | 4.60 - 7.60 % @Temperature 140 - 302 °F |
Modulus of Elasticity | 1.16 - 20.2 GPa | 168 - 2930 ksi |
| 2.50 - 11.6 GPa @Temperature -40.0 - 150 °C | 363 - 1680 ksi @Temperature -40.0 - 302 °F |
Flexural Yield Strength | 29.0 - 800 MPa | 4210 - 116000 psi |
| 89.0 - 380 MPa @Temperature -40.0 - 121 °C | 12900 - 55100 psi @Temperature -40.0 - 250 °F |
Flexural Modulus | 0.724 - 18.5 GPa | 105 - 2680 ksi |
| 2.97 - 12.5 GPa @Temperature -40.0 - 121 °C | 431 - 1810 ksi @Temperature -40.0 - 250 °F |
Flexural Strain at Break | 2.00 - 11.6 % | 2.00 - 11.6 % |
Compressive Yield Strength | 120 - 222 MPa | 17400 - 32200 psi |
| 70.0 - 250 MPa @Temperature -40.0 - 80.0 °C | 10200 - 36300 psi @Temperature -40.0 - 176 °F |
Poissons Ratio | 0.340 - 0.350 | 0.340 - 0.350 |
Shear Modulus | 3.60 - 4.10 GPa | 522 - 595 ksi |
Shear Strength | 60.0 - 85.0 MPa | 8700 - 12300 psi |
Izod Impact, Notched | 0.370 - 3.36 J/cm | 0.693 - 6.30 ft-lb/in |
| 0.700 - 3.84408 J/cm @Temperature -40.0 - 121 °C | 1.31 - 7.20154 ft-lb/in @Temperature -40.0 - 250 °F |
| 1.01441 - 1.33475 J/cm @Temperature -40.0 - -40.0 °C | 1.90041 - 2.50053 ft-lb/in @Temperature -40.0 - -40.0 °F |
| 1.01441 - 1.33475 J/cm @Thickness 3.17 - 3.17 mm | 1.90041 - 2.50053 ft-lb/in @Thickness 0.125 - 0.125 in |
Izod Impact, Unnotched | 0.122 - 5340 J/cm | 0.229 - 10000 ft-lb/in |
Izod Impact, Notched (ISO) | 1.50 - 182 kJ/m² | 0.714 - 86.6 ft-lb/in² |
| 3.00 - 35.0 kJ/m² @Temperature -40.0 - -30.0 °C | 1.43 - 16.7 ft-lb/in² @Temperature -40.0 - -22.0 °F |
Izod Impact, Unnotched (ISO) | 2.60 kJ/m² - NB | 1.24 ft-lb/in² - NB |
| 25.0 kJ/m² - NB @Temperature -30.0 - -30.0 °C | 11.9 ft-lb/in² - NB @Temperature -22.0 - -22.0 °F |
Charpy Impact Unnotched | 0.220 J/cm² - NB | 1.05 ft-lb/in² - NB |
| 0.700 J/cm² - NB @Temperature -40.0 - -20.0 °C | 3.33 ft-lb/in² - NB @Temperature -40.0 - -4.00 °F |
Charpy Impact, Notched | 0.200 J/cm² - NB | 0.952 ft-lb/in² - NB |
| 0.150 - 3.50 J/cm² @Temperature -40.0 - -20.0 °C | 0.714 - 16.7 ft-lb/in² @Temperature -40.0 - -4.00 °F |
Puncture Energy | 2.00 - 14.0 J | 1.48 - 10.3 ft-lb |
| 1.70 - 6.00 J @Temperature -30.0 - -30.0 °C | 1.25 - 4.43 ft-lb @Temperature -22.0 - -22.0 °F |
Coefficient of Friction | 0.150 - 0.610 | 0.150 - 0.610 |
Coefficient of Friction, Static | 0.190 - 0.450 | 0.190 - 0.450 |
Tensile Creep Modulus, 1 hour | 2400 - 92000 MPa | 348000 - 1.33e+7 psi |
Tensile Creep Modulus, 1000 hours | 2000 - 6500 MPa | 290000 - 943000 psi |
Taber Abrasion, mg/1000 Cycles | 0.350 - 25.0 | 0.350 - 25.0 |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 25.0 - 1.00e+18 ohm-cm | 25.0 - 1.00e+18 ohm-cm |
Surface Resistance | 100 - 1.00e+16 ohm | 100 - 1.00e+16 ohm |
Dielectric Constant | 2.50 - 38.0 | 2.50 - 38.0 |
Dielectric Strength | 7.87 - 80.0 kV/mm | 200 - 2030 kV/in |
Dissipation Factor | 0.00500 - 0.850 | 0.00500 - 0.850 |
Dielectric Loss Index | 0.0220 - 0.240 | 0.0220 - 0.240 |
Arc Resistance | 15.0 - 180 sec | 15.0 - 180 sec |
Comparative Tracking Index | 0.000 - 600 V | 0.000 - 600 V |
Hot Wire Ignition, HWI | 15.0 - 60.0 sec | 15.0 - 60.0 sec |
High Amp Arc Ignition, HAI | 120 arcs | 120 arcs |
High Voltage Arc-Tracking Rate, HVTR | 25.4 - 150 mm/min | 1.00 - 5.91 in/min |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 2.50 - 82.0 µm/m-°C | 1.39 - 45.6 µin/in-°F |
| 6.00 - 14.0 µm/m-°C @Temperature 55.0 - 160 °C | 3.33 - 7.78 µin/in-°F @Temperature 131 - 320 °F |
| 20.0 - 31.0 µm/m-°C @Temperature 35.0 - 55.0 °C | 11.1 - 17.2 µin/in-°F @Temperature 95.0 - 131 °F |
| 20.0 - 31.0 µm/m-°C @Thickness 2.00 - 2.00 mm | 11.1 - 17.2 µin/in-°F @Thickness 0.0787 - 0.0787 in |
CTE, linear, Transverse to Flow | 23.0 - 150 µm/m-°C | 12.8 - 83.3 µin/in-°F |
| 110 - 130 µm/m-°C @Temperature 55.0 - 160 °C | 61.1 - 72.2 µin/in-°F @Temperature 131 - 320 °F |
Specific Heat Capacity | 0.350 - 2.43 J/g-°C | 0.0837 - 0.582 BTU/lb-°F |
| 2.20 - 2.28 J/g-°C @Temperature 270 - 270 °C | 0.526 - 0.545 BTU/lb-°F @Temperature 518 - 518 °F |
Thermal Conductivity | 0.200 - 1.64 W/m-K | 1.39 - 11.4 BTU-in/hr-ft²-°F |
| 0.230 - 0.260 W/m-K @Temperature 270 - 270 °C | 1.60 - 1.80 BTU-in/hr-ft²-°F @Temperature 518 - 518 °F |
Melting Point | 178 - 325 °C | 352 - 617 °F |
Crystallization Temperature | 167 - 190 °C | 333 - 374 °F |
Maximum Service Temperature, Air | 65.0 - 288 °C | 149 - 550 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 110 - 305 °C | 230 - 581 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 65.0 - 290 °C | 149 - 554 °F |
Deflection Temperature at 8.0 MPa | 60.0 - 213 °C | 140 - 415 °F |
Vicat Softening Point | 145 - 313 °C | 293 - 595 °F |
Heat Distortion Temperature | 215 - 255 °C | 419 - 491 °F |
Minimum Service Temperature, Air | -60.0 - -20.0 °C | -76.0 - -4.00 °F |
Glass Transition Temp, Tg | 5.00 - 67.0 °C | 41.0 - 153 °F |
Decomposition Temperature | 300 - 350 °C | 572 - 662 °F |
UL RTI, Electrical | 65.0 - 140 °C | 149 - 284 °F |
UL RTI, Mechanical with Impact | 65.0 - 125 °C | 149 - 257 °F |
UL RTI, Mechanical without Impact | 65.0 - 150 °C | 149 - 302 °F |
Flammability, UL94 | HB - 5VA | HB - 5VA |
Flame Spread | 0.000 - 102 mm/min | 0.000 - 4.02 in/min |
Oxygen Index | 21.0 - 39.8 % | 21.0 - 39.8 % |
Glow Wire Test | 500 - 960 °C | 932 - 1760 °F |
Ignition Temperature | 400 - 470 °C | 752 - 878 °F |
|
Processing Properties | Metric | English | Comments |
---|
Processing Temperature | 70.0 - 300 °C | 158 - 572 °F |
Nozzle Temperature | 55.0 - 295 °C | 131 - 563 °F |
Melt Temperature | 210 - 350 °C | 410 - 662 °F |
Mold Temperature | 21.1 - 121 °C | 70.0 - 250 °F |
Drying Temperature | 26.7 - 180 °C | 80.0 - 356 °F |
Moisture Content | 0.00150 - 1.12 % | 0.00150 - 1.12 % |
Dew Point | -40.0 - -17.8 °C | -40.0 - 0.000 °F |
Injection Pressure | 3.45 - 172 MPa | 500 - 25000 psi |
Vent Depth | 0.00127 - 0.00762 cm | 0.000500 - 0.00300 in |