MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Plating Grade
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Plating Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Acrylonitrile Butadiene Styrene (ABS), Plating Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.03 - 2.50 g/cc0.0372 - 0.0903 lb/in³Average value: 1.09 g/cc Grade Count:35
Water Absorption 0.200 - 1.00 %0.200 - 1.00 %Average value: 0.420 % Grade Count:5
Linear Mold Shrinkage 0.00300 - 0.00800 cm/cm0.00300 - 0.00800 in/inAverage value: 0.00541 cm/cm Grade Count:29
Linear Mold Shrinkage, Transverse 0.00300 - 0.00800 cm/cm0.00300 - 0.00800 in/inAverage value: 0.00587 cm/cm Grade Count:8
Melt Flow 1.20 - 45.0 g/10 min1.20 - 45.0 g/10 minAverage value: 13.7 g/10 min Grade Count:34
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 101 - 116101 - 116Average value: 108 Grade Count:22
Ball Indentation Hardness 74.0 - 100 MPa10700 - 14500 psiAverage value: 91.3 MPa Grade Count:6
Tensile Strength, Ultimate 20.0 - 48.0 MPa2900 - 6960 psiAverage value: 38.5 MPa Grade Count:21
Tensile Strength, Yield 36.0 - 63.0 MPa5220 - 9140 psiAverage value: 44.7 MPa Grade Count:27
Elongation at Break 3.00 - 70.0 %3.00 - 70.0 %Average value: 26.0 % Grade Count:27
Elongation at Yield 2.00 - 7.00 %2.00 - 7.00 %Average value: 4.08 % Grade Count:9
Modulus of Elasticity 1.70 - 2.77 GPa247 - 402 ksiAverage value: 2.28 GPa Grade Count:16
Flexural Yield Strength 56.0 - 82.0 MPa8120 - 11900 psiAverage value: 68.1 MPa Grade Count:30
Flexural Modulus 1.96 - 5.47 GPa284 - 793 ksiAverage value: 2.37 GPa Grade Count:36
Izod Impact, Notched 0.230 - 5.82 J/cm0.431 - 10.9 ft-lb/inAverage value: 2.63 J/cm Grade Count:25
 0.5339 - 3.50 J/cm
@Temperature -40.0 - 0.000 °C
1.000 - 6.56 ft-lb/in
@Temperature -40.0 - 32.0 °F
Average value: 1.08 J/cm Grade Count:2
 0.784532 - 0.980 J/cm
@Temperature -30.0 - -30.0 °C
1.46975 - 1.84 ft-lb/in
@Temperature -22.0 - -22.0 °F
Average value: 1.08 J/cm Grade Count:3
 0.784532 - 0.980 J/cm
@Thickness 3.17 - 12.7 mm
1.46975 - 1.84 ft-lb/in
@Thickness 0.125 - 0.500 in
Average value: 1.08 J/cm Grade Count:3
Izod Impact, Unnotched  1.471 - 1.56906 J/cm
@Temperature -30.0 - -30.0 °C
2.756 - 2.93950 ft-lb/in
@Temperature -22.0 - -22.0 °F
Average value: 1.52 J/cm Grade Count:1
 1.471 - 1.56906 J/cm
@Thickness 3.20 - 6.40 mm
2.756 - 2.93950 ft-lb/in
@Thickness 0.126 - 0.252 in
Average value: 1.52 J/cm Grade Count:1
Izod Impact, Notched (ISO) 16.4 - 58.0 kJ/m²7.79 - 27.6 ft-lb/in²Average value: 25.8 kJ/m² Grade Count:10
 7.00 - 41.0 kJ/m²
@Temperature -30.0 - -20.0 °C
3.33 - 19.5 ft-lb/in²
@Temperature -22.0 - -4.00 °F
Average value: 13.9 kJ/m² Grade Count:7
Charpy Impact Unnotched 17.0 J/cm² - NB80.9 ft-lb/in² - NBAverage value: 17.0 J/cm² Grade Count:3
 11.0 - 15.0 J/cm²
@Temperature -30.0 - -30.0 °C
52.4 - 71.4 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 13.0 J/cm² Grade Count:2
Charpy Impact, Notched 1.70 - 5.30 J/cm²8.09 - 25.2 ft-lb/in²Average value: 2.45 J/cm² Grade Count:13
 0.700 - 4.00 J/cm²
@Temperature -30.0 - -20.0 °C
3.33 - 19.0 ft-lb/in²
@Temperature -22.0 - -4.00 °F
Average value: 1.50 J/cm² Grade Count:7
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+14 - 1.00e+16 ohm-cm1.00e+14 - 1.00e+16 ohm-cmAverage value: 5.35e+15 ohm-cm Grade Count:6
Surface Resistance 1.00e+14 - 1.00e+16 ohm1.00e+14 - 1.00e+16 ohmAverage value: 5.27e+15 ohm Grade Count:4
Dielectric Constant 2.90 - 3.002.90 - 3.00Average value: 2.96 Grade Count:3
Dielectric Strength 28.0 - 38.0 kV/mm711 - 965 kV/inAverage value: 33.3 kV/mm Grade Count:4
Dissipation Factor 0.00500 - 0.01500.00500 - 0.0150Average value: 0.00860 Grade Count:3
Comparative Tracking Index 600 V600 VAverage value: 600 V Grade Count:3
 
Thermal PropertiesMetricEnglishComments
CTE, linear 67.0 - 100 µm/m-°C37.2 - 55.6 µin/in-°FAverage value: 85.6 µm/m-°C Grade Count:11
Thermal Conductivity 0.250 - 0.250 W/m-K
@Temperature 30.0 - 260 °C
1.74 - 1.74 BTU-in/hr-ft²-°F
@Temperature 86.0 - 500 °F
Average value: 0.250 W/m-K Grade Count:1
Deflection Temperature at 0.46 MPa (66 psi) 87.8 - 113 °C190 - 235 °FAverage value: 96.5 °C Grade Count:16
Deflection Temperature at 1.8 MPa (264 psi) 76.1 - 203 °C169 - 397 °FAverage value: 92.6 °C Grade Count:35
Vicat Softening Point 90.0 - 115 °C194 - 239 °FAverage value: 101 °C Grade Count:28
UL RTI, Electrical 60.0 - 80.0 °C140 - 176 °FAverage value: 64.0 °C Grade Count:3
UL RTI, Mechanical with Impact 60.0 - 80.0 °C140 - 176 °FAverage value: 64.0 °C Grade Count:3
UL RTI, Mechanical without Impact 60.0 - 80.0 °C140 - 176 °FAverage value: 64.0 °C Grade Count:3
Flammability, UL94 HBHBGrade Count:28
Glow Wire Test 650 - 700 °C1200 - 1290 °FAverage value: 667 °C Grade Count:3
 
Optical PropertiesMetricEnglishComments
Gloss 90.0 - 98.0 %90.0 - 98.0 %Average value: 95.5 % Grade Count:4
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 210 - 274 °C410 - 525 °FAverage value: 228 °C Grade Count:4
Melt Temperature 188 - 274 °C370 - 525 °FAverage value: 221 °C Grade Count:18
Mold Temperature 40.0 - 85.0 °C104 - 185 °FAverage value: 63.0 °C Grade Count:19
Injection Velocity 240 mm/sec9.45 in/secAverage value: 240 mm/sec Grade Count:4
Drying Temperature 70.0 - 93.3 °C158 - 200 °FAverage value: 84.0 °C Grade Count:16
Injection Pressure 4.83 - 150 MPa700 - 21800 psiAverage value: 65.8 MPa Grade Count:10

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Impact Grade, Molded
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Extruded
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Unreinforced, Flame Retardant
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded

O1107 / 77798

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.