Mocom (ALBIS) ALTECH® PA66 B 1000/500 Nylon 66
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, Unreinforced
Material Notes:
Base Polymer: Polyamide 66
Special Features: Injection molding grade
Typical Application: Various
Information provided by Albis Plastics
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.13
g/cc
0.0408
lb/in³
ISO 1183
Linear Mold Shrinkage, Flow
0.010
-
0.012
cm/cm
@Time 86400 sec
0.010
-
0.012
in/in
@Time 24.0 hour
ISO 294-4
Linear Mold Shrinkage, Transverse
0.012
-
0.014
cm/cm
@Time 86400 sec
0.012
-
0.014
in/in
@Time 24.0 hour
ISO 294-4
Storage Temperature
<=
30.0
°C
<=
86.0
°F
dry, protected from light
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
75.0
MPa
10900
psi
ISO 527
Elongation at Break
10 %
10 %
ISO 527
Tensile Modulus
3.20
GPa
464
ksi
ISO 527
Flexural Strength
110
MPa
16000
psi
ISO 178
Flexural Modulus
2.80
GPa
406
ksi
ISO 178
Charpy Impact Unnotched
NB
NB
ISO 179/1eU
Charpy Impact, Notched
0.500
J/cm²
2.38
ft-lb/in²
ISO 179/1eA
Thermal Properties
Metric
English
Comments
Melting Point
263
°C
505
°F
ISO 11357
Deflection Temperature at 1.8 MPa (264 psi)
70.0
°C
158
°F
ISO 75-1/-2
Vicat Softening Point
240
°C
464
°F
B50; ISO 306
Processing Properties
Metric
English
Comments
Melt Temperature
270
-
290
°C
518
-
554
°F
Injection molding
Mold Temperature
60.0
-
90.0
°C
140
-
194
°F
Injection molding
Drying Temperature
80.0
°C
@Time 7200 - 43200 sec
176
°F
@Time 2.00 - 12.0 hour
in a dry air (desiccant) dryer
Descriptive Properties
Base Polymer
Polyamide 66
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PALBIS8756 / 242815
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.