MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Plenco 301 Black Impact Grade Woodflour/Flock Filled Phenolic Molding Compound  (discontinued **)
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Phenolic; Phenolic, Novolac, Impact Grade, Filled

Material Notes: Plaslok 301 is a two-stage, woodflour and flock-filled phenolic molding compound. It has broad molding latitude combined with good electrical properties and improved impact strength. It is particularly suited for mechanical parts with thin sections that require wheelabrating, staking or pulling of inserts.

Data provided by Plaslok Corporation.

Plaslok Corporation was purchased by Plastics Engineering Company in March 2000. The Plaslok name is no longer used on any products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.38 g/cc0.0499 lb/in³ASTM D792
Apparent Bulk Density 0.520 g/cc0.0188 lb/in³ASTM D1895
Water Absorption 1.0 %1.0 %ASTM D570
Linear Mold Shrinkage 0.0070 cm/cm0.0070 in/inCompression; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 41.0 MPa5950 psiASTM D638
Flexural Yield Strength 76.0 MPa11000 psiASTM D790
Flexural Modulus 8.30 GPa1200 ksiASTM D790
Compressive Yield Strength 221 MPa32100 psiASTM D695
Izod Impact, Notched 0.250 J/cm0.468 ft-lb/inASTM D256
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+12 ohm-cm1.00e+12 ohm-cmASTM D257
Dielectric Constant  4.2
@Frequency 1e+6 Hz
4.2
@Frequency 1e+6 Hz
ASTM D150
 6.8
@Frequency 60 Hz
6.8
@Frequency 60 Hz
ASTM D150
Dielectric Strength 11.8 kV/mm300 kV/inASTM D149
Dissipation Factor  0.040
@Frequency 1e+6 Hz
0.040
@Frequency 1e+6 Hz
ASTM D150
 0.090
@Frequency 60 Hz
0.090
@Frequency 60 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 177 °C351 °FASTM D648

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Plenco 6527 Phenolic, Granular, Injection Molded
Röchling Glastic BMC 1603 GTP Glass-Reinforced Polyester
Plenco 7300 Phenolic, Nodular, Injection Molded
Plenco 202 Black General Purpose Woodflour Filled Phenolic Molding Compound
Owens Corning Glass Fiber Reinforced Polyester (Pultruded), 55 wt.% glass

PLEO911 / 50800

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.