MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Assab Steels DIEVAR Hot Work Steel
Categories: Metal; Ferrous Metal; Chrome-moly Steel; Tool Steel; Hot Work Steel

Material Notes: DIEVAR is a high performance chromium-molybdenum-vanadium alloyed hot work tool steel which offers a very good resistance to heat checking, gross checking, hot wear and plastic deformation. DIEVAR is characterized by:
  • Excellent toughness and ductility in all directions
  • Good temper resistance
  • Good high-temperature strength
  • Excellent hardenability
  • Good dimensional stability throughout heat treatment and coating operations

Applications: Die casting, forging, and extrusion

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.78 g/cc0.281 lb/in³
 7.58 g/cc
@Temperature 800 °C
0.274 lb/in³
@Temperature 1470 °F
 7.67 g/cc
@Temperature 399 °C
0.277 lb/in³
@Temperature 750 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 2626Hardness during tempering. At tempering temperature (2+ 2h) 700°C. Austenitizing temperature 1025°C (1875°F)
 3131Temper resistance. 10 hour holding time at 650°C (1200°F).
 3232Temper resistance. 100 hour holding time at 600°C (1110°F).
 3333Hardness during tempering. At tempering temperature (2+ 2h) 650°C. Austenitizing temperature 1000°C (1830°F)
 4040Temper resistance. 1 hour holding time at 650°C (1200°F).
 4242Temper resistance. 100 hour holding time at 550°C (1020°F).
 4242Temper resistance. 10 hour holding time at 600°C (1110°F).
 4545Temper resistance. 10 hour holding time at 550°C (1020°F).
 4545Temper resistance. 1 hour holding time at 550°C (1020°F).
 4545Temper resistance. 1 hour holding time at 600°C (1110°F).
 4545Temper resistance. 1-100 hour holding time at 500°C (930°F)
 5151Hardness during tempering. At tempering temperature (2+ 2h) 400°C. Austenitizing temperature 1000°C (1830°F)
 5252Hardness during tempering. At tempering temperature (2+ 2h) 400°C. Austenitizing temperature 1025°C (1875°F)
 5252Hardness during tempering. At tempering temperature (2+ 2h) 550°C. Austenitizing temperature 1000°C (1830°F)
 50 - 5450 - 54Hardness before tempering. Austenitizing temperature: 1000°C (1830°F). Soaking time 30 minutes.
 5353tempering temperature (2+ 2h) 550°C. Austenitizing temperature 1025°C (1875°F)
 5353Hardness during tempering. At tempering temperature (2+ 2h) 150°C. Austenitizing temperature 1000°C (1830°F)
 54541000°C (1830°F) austenitizing temperature.
 53 - 5753 - 57Hardness before tempering. Austenitizing temperature: 1025°C (1875°F). Soaking time 30 minutes.
 5555Hardness during tempering. At tempering temperature (2+ 2h) 150°C. Austenitizing temperature 1025°C (1875°F)
 56561025°C (1877°F) austenitizing temperature.
 57571052°C (1920°F) austenitizing temperature
Tensile Strength at Break  1100 MPa
@Temperature 500 °C
160000 psi
@Temperature 932 °F
Rm. Short transverse direction.
 1450 MPa
@Temperature 100 °C
210000 psi
@Temperature 212 °F
Rm. Short transverse direction.
Tensile Strength, Ultimate 1480 MPa215000 psiRm. short transverse direction. 44 HRC.
 1640 MPa238000 psiRm. short transverse direction. 48 HRC.
 1900 MPa
@Temperature 23.0 °C
276000 psi
@Temperature 73.4 °F
Tensile Strength, Yield 1210 MPa175000 psiRp02. short transverse direction. 44 HRC.
 1380 MPa200000 psiRp02. short transverse direction. 48 HRC.
 900 MPa
@Temperature 500 °C
131000 psi
@Temperature 932 °F
Rp02. Short transverse direction.
 1200 MPa
@Temperature 100 °C
174000 psi
@Temperature 212 °F
Rp02. Short transverse direction.
 1560 MPa
@Temperature 23.0 °C
226000 psi
@Temperature 73.4 °F
Elongation at Break 12.5 %12.5 %short transverse direction. 52 HRC
 13 %13 %short transverse direction. 44 HRC
 13 %13 %short transverse direction. 48 HRC
 11 %
@Temperature 200 °C
11 %
@Temperature 392 °F
short transverse direction
 15 %
@Temperature 400 °C
15 %
@Temperature 752 °F
short transverse direction.
 18 %
@Temperature 600 °C
18 %
@Temperature 1110 °F
short transverse direction.
Reduction of Area 52 %52 %short transverse direction. 52 HRC
 55 %55 %short transverse direction. 44 HRC
 55 %55 %short transverse direction. 48 HRC
 50 %
@Temperature 200 °C
50 %
@Temperature 392 °F
short transverse direction
 60 %
@Temperature 400 °C
60 %
@Temperature 752 °F
short transverse direction.
 82 %
@Temperature 600 °C
82 %
@Temperature 1110 °F
short transverse direction
Modulus of Elasticity 210 GPa30500 ksi
 145 GPa
@Temperature 800 °C
21000 ksi
@Temperature 1470 °F
 180 GPa
@Temperature 400 °C
26100 ksi
@Temperature 752 °F
Charpy Impact 28.0 J20.7 ft-lbV notch. Short transverse direction. 700°C tempering temperature (2 + 2h).
 47.0 J34.7 ft-lbV notch. Short transverse direction. 600°C tempering temperature (2 + 2h).
 51.0 J37.6 ft-lbV notch. Short transverse direction. 400°C tempering temperature (2 + 2h).
 55.0 J40.6 ft-lbV notch. Short transverse direction. 200°C tempering temperature (2 + 2h).
 39.0 J
@Temperature 100 °C
28.8 ft-lb
@Temperature 212 °F
V-notch. Short transverse direction. 50 HRC
 45.0 J
@Temperature 100 °C
33.2 ft-lb
@Temperature 212 °F
V-notch. Short transverse direction. 47 HRC
 55.0 J
@Temperature 100 °C
40.6 ft-lb
@Temperature 212 °F
V-notch. Short transverse direction. 45 HRC
 70.0 J
@Temperature 250 °C
51.6 ft-lb
@Temperature 482 °F
V-notch. Short transverse direction. 47 HRC
 70.0 J
@Temperature 250 °C
51.6 ft-lb
@Temperature 482 °F
V-notch. Short transverse direction. 50 HRC
 91.0 J
@Temperature 250 °C
67.1 ft-lb
@Temperature 482 °F
V-notch. Short transverse direction. 45 HRC
 97.0 J
@Temperature 400 °C
71.5 ft-lb
@Temperature 752 °F
V-notch. Short transverse direction. 47 HRC
 105 J
@Temperature 400 °C
77.4 ft-lb
@Temperature 752 °F
V-notch. Short transverse direction. 45 HRC
 110 J
@Temperature 400 °C
81.1 ft-lb
@Temperature 752 °F
V-notch. Short transverse direction. 50 HRC
Impact Test >= 300 J
@Temperature 23.0 °C
>= 221 ft-lb
@Temperature 73.4 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.7 µm/m-°C
@Temperature 20.0 - 400 °C
7.06 µin/in-°F
@Temperature 68.0 - 752 °F
 13.3 µm/m-°C
@Temperature 20.0 - 600 °C
7.39 µin/in-°F
@Temperature 68.0 - 1110 °F
Thermal Conductivity  31.0 W/m-K
@Temperature 400 °C
215 BTU-in/hr-ft²-°F
@Temperature 752 °F
 32.0 W/m-K
@Temperature 600 °C
222 BTU-in/hr-ft²-°F
@Temperature 1110 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bohler-Uddeholm UDDEHOLM DIEVAR® Hot Work Tool Steel
Aluminum A383.0-F Die Casting Alloy
Overview of materials for Chrome-moly Steel
Assab Steels QRO 90 SUPREME Hot Work Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPERIOR (Premium AISI H13) Hot Work Tool Steel

NASSAB14 / 15032

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.