MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales
metalmen Is Your Direct to US Manufacturing Source for High Purity Metals

Copper, Cu; Cold-Worked
Categories: Metal; Nonferrous Metal; Copper Alloy; Pure Element

Material Notes: Cold-worked applies only to tensile and/or hardness values; other property values are typical of the element. This entry is for pure Cu, MatWeb also has entries for many alloys.

In general, copper alloys exhibit good to excellent corrosion resistance and high thermal conductivity and very high electrical conductivity. Pure copper's electrical conductivity is so high that many metals are measured against it in the form of the IACS (International Annealed Copper Standard). Applications include architectural uses, coinage, condenser/heat exchangers, plumbing, radiator cores, musical instruments, locks, fasteners, hinges, ammunition components, and electrical connectors. Small amounts of alloying elements are often added to copper to improve certain characteristics. Alloying can increase or reduce the strength, hardness, electrical and thermal conductivity, corrosion resistance, or change the color. Common primary alloying elements include tin (resulting in bronze) or zinc (resulting in brass).

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.96 g/cc0.324 lb/in³
 7.764 g/cc
@Temperature 1300 °C
0.2805 lb/in³
@Temperature 2370 °F
 7.846 g/cc
@Temperature 1200 °C
0.2835 lb/in³
@Temperature 2190 °F
 7.924 g/cc
@Temperature 1100 °C
0.2863 lb/in³
@Temperature 2010 °F
 8.93 g/cc
@Temperature 20.0 °C
0.323 lb/in³
@Temperature 68.0 °F
 
Chemical PropertiesMetricEnglishComments
Atomic Mass 65.54665.5461995
Atomic Number 2929
Thermal Neutron Cross Section 3.8 barns/atom3.8 barns/atom
X-ray Absorption Edge 1.38 Å1.38 ÅK
 11.269 Å11.269 ÅLI
 12.994 Å12.994 ÅLII
 13.2578 Å13.2578 ÅLIII
Electrode Potential -0.520 V-0.520 Vmonovalent
 -0.340 V-0.340 Vdivalent
Electronegativity 1.91.9Pauling
Ionic Radius 0.720 Å0.720 ÅCrystal Ionic Radius for Valence +2
 0.960 Å0.960 ÅCrystal Ionic Radius for Valence +1
Electrochemical Equivalent 1.185 g/A/h1.185 g/A/hdivalent
 2.38 g/A/h2.38 g/A/hmonovalent
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 8989Converted from Vickers for 500 kg load/10 mm ball Brinell test.
Hardness, Rockwell A 3535Converted from Vickers.
Hardness, Rockwell B 5151Converted from Vickers.
Hardness, Vickers 100100
Modulus of Elasticity 110 GPa16000 ksi
Bulk Modulus 140 GPa20300 ksi
Poissons Ratio 0.350.35
Shear Modulus 46.0 GPa6670 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000170 ohm-cm0.00000170 ohm-cm
Magnetic Susceptibility -8.00e-8-8.00e-8cgs/g
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 204.8 J/g88.10 BTU/lb
Heat of Vaporization 5234 J/g2252 BTU/lb
CTE, linear  16.4 µm/m-°C
@Temperature 20.0 - 100 °C
9.11 µin/in-°F
@Temperature 68.0 - 212 °F
 18.5 µm/m-°C
@Temperature 250 °C
10.3 µin/in-°F
@Temperature 482 °F
 20.2 µm/m-°C
@Temperature 500 °C
11.2 µin/in-°F
@Temperature 932 °F
 24.8 µm/m-°C
@Temperature 925 °C
13.8 µin/in-°F
@Temperature 1700 °F
Specific Heat Capacity 0.385 J/g-°C0.0920 BTU/lb-°F
Thermal Conductivity 385 W/m-K2670 BTU-in/hr-ft²-°F
 357 W/m-K
@Temperature 727 °C
2480 BTU-in/hr-ft²-°F
@Temperature 1340 °F
 398 W/m-K
@Temperature 27.0 °C
2760 BTU-in/hr-ft²-°F
@Temperature 80.6 °F
 401 W/m-K
@Temperature 0.000 °C
2780 BTU-in/hr-ft²-°F
@Temperature 32.0 °F
 483 W/m-K
@Temperature -173 °C
3350 BTU-in/hr-ft²-°F
@Temperature -279 °F
 10500 W/m-K
@Temperature -253 °C
72900 BTU-in/hr-ft²-°F
@Temperature -423 °F
 19600 W/m-K
@Temperature -263 °C
136000 BTU-in/hr-ft²-°F
@Temperature -441 °F
Melting Point 1083.2 - 1083.6 °C1981.8 - 1982.5 °F
Boiling Point 2562 °C4644 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.15
@Wavelength >=655 nm,
Temperature 807 °C
0.15
@Wavelength >=655 nm,
Temperature 1480 °F
polished
Reflection Coefficient, Visible (0-1) 0.630.63
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 100 %100 %
 
Descriptive Properties
CAS Number7440-50-8

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Copper, Cu; Annealed
Copper, Cu; Cold Drawn
Aluminum, Al
Gold, Au
Silver, Ag

AMECu01 / 29

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.