MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Domo TECHNYL® B 738 MX15 PA 66/6, 15% Mineral Fiber Reinforced, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, Mineral Reinforced

Material Notes: Description: TECHNYL B 738 MX15 is a copolyamide 6.6, reinforced with 15% of mineral filler, for injection molding. This product is available in black and grey colors.

Key Properties: Good surface aspect; Mechanical performance

Benefits: This grade offers good mechanical Properties, good superficial aspect and dimensional stability.

Applications: It is indicated for automotive and electrical industry. Ex.: Wheel Cover

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.22 g/cc0.0441 lb/in³ISO 1183/A
Water Absorption 1.17 %
@Time 86400 sec
1.17 %
@Time 24.0 hour
ISO 62
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 59.0 MPa8560 psiISO 527 Type 1A
Elongation at Break 3.0 %3.0 %ISO 527 Type 1A
Tensile Modulus 4.30 GPa624 ksiISO 527 Type 1A
Flexural Strength 100 MPa14500 psiISO 178
Flexural Modulus 3.70 GPa537 ksiISO 178
Charpy Impact Unnotched 6.00 J/cm²28.6 ft-lb/in²ISO 179/1eU
 
Thermal PropertiesMetricEnglishComments
Melting Point 244 °C471 °FISO 11357
 
Processing PropertiesMetricEnglishComments
Processing Temperature 250 - 255 °C482 - 491 °FCompression zone
 255 - 265 °C491 - 509 °FMixing zone
Feed Temperature 245 - 250 °C473 - 482 °F
Mold Temperature 60.0 - 90.0 °C140 - 194 °F
Drying Temperature 80.0 °C176 °F
Moisture Content <= 0.20 %<= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
IN-738 Cast Nickel Superalloy
Special Metals INCONEL® alloy 783 Ni-Co-Fe Alloy
Nye Lubricants 738 (RL) Synthetic Oil
Nimocast 738 Superalloy
Esstech X-738-0000 Ethoxylated Bis Phenol A Dimethacrylate, C83H144O34

PSOLVAY856 / 218584

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.