MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Overview of materials for Acrylonitrile Butadiene Styrene (ABS), 10% Glass Fiber Filled
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), 10% Glass Fiber Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Acrylonitrile Butadiene Styrene (ABS), 10% Glass Fiber Filled". Specific grades with glass content between 5% and 14% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.06 - 1.40 g/cc0.0383 - 0.0506 lb/in³Average value: 1.13 g/cc Grade Count:88
Filler Content 5.00 - 15.0 %5.00 - 15.0 %Average value: 9.72 % Grade Count:17
Water Absorption 0.100 - 0.300 %0.100 - 0.300 %Average value: 0.224 % Grade Count:24
Maximum Moisture Content 0.0200 - 0.2000.0200 - 0.200Average value: 0.0729 Grade Count:7
Linear Mold Shrinkage 0.00100 - 0.00900 cm/cm0.00100 - 0.00900 in/inAverage value: 0.00323 cm/cm Grade Count:72
Linear Mold Shrinkage, Transverse 0.00200 - 0.00600 cm/cm0.00200 - 0.00600 in/inAverage value: 0.00300 cm/cm Grade Count:6
Melt Flow 0.100 - 96.0 g/10 min0.100 - 96.0 g/10 minAverage value: 10.4 g/10 min Grade Count:48
Ash 9.70 - 10.0 %9.70 - 10.0 %Average value: 9.93 % Grade Count:4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 55.0 - 10255.0 - 102Average value: 73.4 Grade Count:5
Hardness, Rockwell R 55.0 - 12055.0 - 120Average value: 109 Grade Count:27
Tensile Strength, Ultimate 26.0 - 102 MPa3770 - 14800 psiAverage value: 60.5 MPa Grade Count:59
 28.0 - 46.0 MPa
@Temperature 60.0 - 90.0 °C
4060 - 6670 psi
@Temperature 140 - 194 °F
Average value: 37.0 MPa Grade Count:1
Tensile Strength, Yield 28.0 - 88.3 MPa4060 - 12800 psiAverage value: 59.3 MPa Grade Count:43
Elongation at Break 2.00 - 10.0 %2.00 - 10.0 %Average value: 3.73 % Grade Count:64
Elongation at Yield 1.90 - 6.00 %1.90 - 6.00 %Average value: 3.03 % Grade Count:10
Modulus of Elasticity 2.50 - 5.88 GPa363 - 853 ksiAverage value: 3.80 GPa Grade Count:25
Flexural Yield Strength 57.0 - 155 MPa8270 - 22500 psiAverage value: 91.0 MPa Grade Count:78
Flexural Modulus 2.34 - 6.54 GPa340 - 949 ksiAverage value: 3.78 GPa Grade Count:85
Izod Impact, Notched 0.490 - 1.80 J/cm0.919 - 3.37 ft-lb/inAverage value: 0.790 J/cm Grade Count:71
 0.450 - 1.50 J/cm
@Temperature -40.0 - 0.000 °C
0.843 - 2.81 ft-lb/in
@Temperature -40.0 - 32.0 °F
Average value: 0.579 J/cm Grade Count:2
 0.300 - 0.500 J/cm
@Temperature -30.0 - 0.000 °C
0.562 - 0.937 ft-lb/in
@Temperature -22.0 - 32.0 °F
Average value: 0.579 J/cm Grade Count:1
 0.300 - 0.500 J/cm
@Thickness 3.20 - 3.20 mm
0.562 - 0.937 ft-lb/in
@Thickness 0.126 - 0.126 in
Average value: 0.579 J/cm Grade Count:1
Izod Impact, Unnotched 2.14 - 3.47 J/cm4.00 - 6.50 ft-lb/inAverage value: 2.92 J/cm Grade Count:20
Izod Impact, Notched (ISO) 5.00 - 16.0 kJ/m²2.38 - 7.61 ft-lb/in²Average value: 8.00 kJ/m² Grade Count:9
Charpy Impact Unnotched 2.00 - 2.70 J/cm²9.52 - 12.8 ft-lb/in²Average value: 2.23 J/cm² Grade Count:3
Charpy Impact, Notched 0.600 - 1.40 J/cm²2.86 - 6.66 ft-lb/in²Average value: 0.808 J/cm² Grade Count:12
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+9 - 1.00e+16 ohm-cm1.00e+9 - 1.00e+16 ohm-cmAverage value: 4.69e+15 ohm-cm Grade Count:18
Surface Resistance 1.00e+10 - 1.00e+14 ohm1.00e+10 - 1.00e+14 ohmAverage value: 6.67e+13 ohm Grade Count:6
Dielectric Constant 3.00 - 3.303.00 - 3.30Average value: 3.17 Grade Count:3
Dielectric Strength 15.7 - 30.0 kV/mm400 - 762 kV/inAverage value: 20.1 kV/mm Grade Count:13
Dissipation Factor 0.00800 - 0.02000.00800 - 0.0200Average value: 0.0127 Grade Count:3
Arc Resistance 60.0 - 180 sec60.0 - 180 secAverage value: 107 sec Grade Count:3
Comparative Tracking Index 175 - 500 V175 - 500 VAverage value: 308 V Grade Count:3
 
Thermal PropertiesMetricEnglishComments
CTE, linear 23.0 - 57.6 µm/m-°C12.8 - 32.0 µin/in-°FAverage value: 43.0 µm/m-°C Grade Count:11
Deflection Temperature at 0.46 MPa (66 psi) 93.3 - 112 °C200 - 233 °FAverage value: 101 °C Grade Count:35
Deflection Temperature at 1.8 MPa (264 psi) 80.0 - 129 °C176 - 264 °FAverage value: 97.4 °C Grade Count:74
Vicat Softening Point 95.0 - 135 °C203 - 275 °FAverage value: 106 °C Grade Count:19
UL RTI, Electrical 50.0 - 60.0 °C122 - 140 °FAverage value: 56.0 °C Grade Count:3
UL RTI, Mechanical with Impact 50.0 - 60.0 °C122 - 140 °FAverage value: 56.0 °C Grade Count:3
UL RTI, Mechanical without Impact 50.0 - 60.0 °C122 - 140 °FAverage value: 56.0 °C Grade Count:3
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:49
 
Processing PropertiesMetricEnglishComments
Processing Temperature 180 - 260 °C356 - 500 °FAverage value: 213 °C Grade Count:10
Nozzle Temperature 210 - 274 °C410 - 525 °FAverage value: 239 °C Grade Count:11
Melt Temperature 188 - 277 °C370 - 530 °FAverage value: 228 °C Grade Count:28
Mold Temperature 20.0 - 100 °C68.0 - 212 °FAverage value: 66.3 °C Grade Count:38
Drying Temperature 70.0 - 104 °C158 - 220 °FAverage value: 84.2 °C Grade Count:32
Moisture Content 0.0200 - 0.150 %0.0200 - 0.150 %Average value: 0.0878 % Grade Count:9
Dew Point -17.8 °C0.000 °FAverage value: -17.8 °C Grade Count:4
Injection Pressure 4.83 - 150 MPa700 - 21800 psiAverage value: 81.6 MPa Grade Count:13
Vent Depth 0.00254 cm0.00100 inAverage value: 0.00254 cm Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), 20% Glass Fiber Filled
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), 30% Glass Fiber Filled
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), 40% Glass Fiber Filled
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), 10% Carbon Fiber Filled

O1111 / 77801

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.