MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Asahi Kasei Leona™ 14025 Polyamide 66, Heat Stabilized
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Heat Stabilized

Material Notes: Applications: Automotive parts, electrical & electronic parts, parts for office furnishings.

Information provided by Asahi Kasei Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³Dry as Molded; ISO 1183
 2.50 g/cc0.0903 lb/in³Conditioned at 50% RH
Linear Mold Shrinkage, Flow 0.013 - 0.020 cm/cm0.013 - 0.020 in/inAsahi Kasei
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 5555Conditioned at 50% RH; ISO 2039
 8080Dry as Molded; ISO 2039
Hardness, Rockwell R 108108Conditioned; ISO 2039
 120120Dry as Molded; ISO 2039
Tensile Strength 57.0 MPa8270 psiConditioned at 50% RH; ASTM D638
 79.0 MPa11500 psiDry as Molded; ASTM D638
Tensile Strength, Yield 52.0 MPa7540 psiConditioned at 50% RH; ISO 527
 82.0 MPa11900 psiDry as Molded; ISO 527
Elongation at Break >= 100 %>= 100 %Conditioned at 50% RH; ISO 527
Elongation at Yield  4.0 %
@Temperature 23.0 °C
4.0 %
@Temperature 73.4 °F
50% RH; ISO 527
 24 %
@Temperature 23.0 °C
24 %
@Temperature 73.4 °F
50% RH; ISO 527
Tensile Modulus 1.20 GPa174 ksiConditioned at 50% RH; ISO 527
 3.00 GPa435 ksiDry as Molded; ISO 527
Flexural Strength 42.0 MPa6090 psiConditioned at 50% RH
 113 MPa16400 psiDry as Molded
Flexural Modulus 1.10 GPa160 ksiConditioned at 50% RH; ISO 178
 2.70 GPa392 ksiDry as Molded; ISO 178
Izod Impact, Notched 0.390 J/cm0.731 ft-lb/inDry as Molded; ASTM D256
 1.47 J/cm2.75 ft-lb/inConditioned at 50% RH; ASTM D256
Charpy Impact Unnotched NBNBConditioned at 50% RH; ISO 179
 NBNBDry as Molded; ISO 179
Charpy Impact, Notched 0.600 J/cm²2.86 ft-lb/in²Dry as Molded; ISO 179
 1.50 J/cm²7.14 ft-lb/in²Conditioned at 50% RH; ISO 179
Taber Abrasion, mg/1000 Cycles 7.07.0Conditioned at 50% RH; ASTM D1044
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmDry as Molded; IEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmDry as Molded; IEC 60093
Dielectric Strength 20.0 kV/mm508 kV/inDry as Molded; IEC 60243
Comparative Tracking Index 525 V
@Thickness 3.00 mm
525 V
@Thickness 0.118 in
Dry as Molded; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 80.0 µm/m-°C44.4 µin/in-°FDry as Molded; ASTMD 696
Specific Heat Capacity 1.67 J/g-°C0.399 BTU/lb-°FDry as Molded
Thermal Conductivity 0.200 W/m-K1.39 BTU-in/hr-ft²-°FDry as Molded
Deflection Temperature at 0.46 MPa (66 psi) 190 °C374 °FDry as Molded; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C158 °FDry as Molded; ISO 75
Flammability, UL94 V-2
@Thickness 0.750 mm
V-2
@Thickness 0.0295 in
Dry as Molded
Oxygen Index 26 %26 %Dry as Molded; ASTM D2863
Glow Wire Flammability Index 960 °C
@Thickness 3.00 mm
1760 °F
@Thickness 0.118 in
Dry as Molded; IEC 60695-2-12

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman ComAlloy Hiloy® 612 Nylon 6, Glass Reinforced, UL
Asahi Kasei Leona™ 13005 Polyamide 66, General Purpose
Asahi Kasei Leona™ 13G15 Polyamide 66, GF Reinforced
Asahi Kasei Leona™ 13G50 Polyamide 66, GF Reinforced
Asahi Kasei Leona™ 90G33 Polyamide 66, GF Reinforced

PASAHI8122 / 221149

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.