MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Samyang Tripet® 2550GN30 Polyethylene Terephthalate, 30% Glass Fiber Reinforced, Flame Retardant
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), Glass Fiber Filled, Flame Retardant

Material Notes: TRIPET® has excellent heat resistance, good surface, chemical resistance and high electrical performance.

Applications:

  • Coil Bobbin
  • Connector
  • Motor Housing
  • Lamp Housing
  • Relay Base
  • Iron body

All information provided by Samyang

Key Words: PET
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.61 g/cc1.61 g/ccASTM D792
Water Absorption 0.10 %
@Time 86400 sec
0.10 %
@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage 0.0020 - 0.0040 cm/cm
@Thickness 3.00 mm
0.0020 - 0.0040 in/in
@Thickness 0.118 in
ASTM D955
Melt Flow 45 g/10 min
@Load 5.00 kg,
Temperature 265 °C
45 g/10 min
@Load 11.0 lb,
Temperature 509 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 114114ASTM D785
Tensile Strength, Yield 147 MPa21300 psiASTM D638
Elongation at Break 6.0 %6.0 %ASTM D638
Flexural Yield Strength 221 MPa32000 psiASTM D790
Flexural Modulus 8.83 GPa1280 ksiASTM D790
Izod Impact, Unnotched 0.883 J/cm
@Thickness 3.17 mm
1.65 ft-lb/in
@Thickness 0.125 in
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmASTM D257
Dielectric Constant 3.8
@Frequency 1e+6 Hz
3.8
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 20.0 kV/mm508 kV/inASTM D149
Dissipation Factor 0.017
@Frequency 1e+6 Hz
0.017
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 80 sec80 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear 30.0 µm/m-°C16.7 µin/in-°FASTM D696
Melting Point 255 °C491 °F
Deflection Temperature at 0.46 MPa (66 psi) 245 °C473 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 220 °C428 °FASTM D648
Flammability, UL94 V-0
@Thickness 1.59 mm
V-0
@Thickness 0.0625 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
SK Chemicals SKYPET® BL8450 Specially Formulated PET Copolymer Resin
Toyobo VYLOPET® EMC133 Injection Molding Polyester Resin, Hydrolysis Resistant
Lotte Advanced Materials Infino® AE-2030 PC/PET, General Purpose
SABIC HC 050 Amorphous Polyethylene Terephthalate
Tempia Polylactic acid (PLA) Resin

PSAMY021 / 88103

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.