MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

INEOS Styrolution PS 576H HIPS
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Impact Modified

Material Notes: Styrolution PS 576H is a high gloss, high impact polystyrene with a good flow and good heat resistance.
  • High gloss HIPS
  • Good flow and heat resistance
  • HIPS with good balance of mechanical properties and surface gloss

Information provided by Styrolution

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ISO 1183
Moisture Absorption at Equilibrium <= 0.10 %
@Temperature 23.0 °C
<= 0.10 %
@Temperature 73.4 °F
50% RH; ISO 62
Water Absorption at Saturation <= 0.10 %
@Temperature 23.0 °C
<= 0.10 %
@Temperature 73.4 °F
ISO 62
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inISO 294-4
Melt Flow 5.5 g/10 min
@Load 5.00 kg,
Temperature 200 °C
5.5 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 83.0 MPa12000 psiISO 2039-1
Tensile Strength, Yield 30.0 MPa4350 psiISO 527
Elongation at Break 30 %30 %ISO 527
Elongation at Yield 1.6 %1.6 %ISO 527
Tensile Modulus 2.05 GPa297 ksiISO 527
Flexural Strength 44.0 MPa6380 psiISO 178
Flexural Modulus 2.10 GPa305 ksiISO 178
Izod Impact, Notched (ISO) 10.0 kJ/m²4.76 ft-lb/in²ISO 180/A
Charpy Impact Unnotched  7.00 J/cm²
@Temperature -30.0 °C
33.3 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 12.0 J/cm²
@Temperature 23.0 °C
57.1 ft-lb/in²
@Temperature 73.4 °F
ISO 179
Charpy Impact, Notched 1.30 J/cm²6.19 ft-lb/in²ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+18 ohm-cm>= 1.00e+18 ohm-cmIEC 60093
Surface Resistance >= 1.00e+13 ohm>= 1.00e+13 ohmIEC 60093
Dielectric Constant 2.5
@Frequency 100 Hz
2.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 155 kV/mm
@Thickness 1.50 mm
3940 kV/in
@Thickness 0.0591 in
Short Time; IEC 60243-1
Dissipation Factor 0.00040
@Frequency 1e+6 Hz
0.00040
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesMetricEnglishComments
CTE, linear 100 µm/m-°C55.6 µin/in-°FISO 11359
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °C190 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 78.0 °C172 °FISO 75
Vicat Softening Point  90.0 °C
@Load 5.10 kg
194 °F
@Load 11.2 lb
50°C/h; ISO 306
 98.0 °C
@Load 1.02 kg
208 °F
@Load 2.25 lb
50°C/h; ISO 306
 
Optical PropertiesMetricEnglishComments
Gloss 70 %70 %Specular Gloss, 60°; ASTM D 523
 
Processing PropertiesMetricEnglishComments
Melt Temperature 180 - 260 °C356 - 500 °FISO 294
Mold Temperature 10.0 - 60.0 °C50.0 - 140 °FISO 294
Injection Velocity 200 mm/sec7.87 in/secISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chevron Phillips MA5350 HIPS - High Impact Polystyrene
Dow AIM® 4800 High Impact Styrenic Resin
INEOS Styrolution PS 476L HIPS
Chevron Phillips MA9545 HIPS - High Impact Polystyrene
Chevron Phillips MD6800 HIPS - High Impact Polystyrene

PBASG1093 / 159639

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.