MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Avient Versollan™ OM 1255NX-1 Thermoplastic Elastomer (TPE)
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Versollan™ OM 1255NX-1 is a high performance TPU alloy designed for thin-wall overmolding onto polycarbonate (PC), ABS, PC/ABS and copolyester substrates. - Improved Grip with Matte, Rubbery Finish - Superior Adhesion to PC, ABS, PC/ABS, PC/PBT and Copolyester

Color concentrates with ethyl vinyl acetate (EVA) or polyether-based urethane carriers are most suitable for coloring Versollan™ OM 1255NX-1. Typical letdown ratios are 50:1 to 25:1 - loading levels should be as low as possible to minimize the effect on hardness. A high color match consistency can be obtained by the use of precolored compounds available from GLS. Polypropylene (PP) based color concentrates are not recommended because they significantly affect adhesion of the TPE to the substrate. Concentrates based on TPE should not be used. The final determination of color concentrate suitability should be determined by customer trials. Purge thoroughly before and after use of this product with a low flow (0.5 - 2.5 MFR) polyethylene (PE) or polypropylene (PP). Regrind levels up to 20% can be used with Versollan™ OM 1255NX-1 with minimal property loss, provided that the regrind is free of contamination. To minimize losses during molding, the melt temperature should remain as low as possible. The final determination of regrind effectiveness should be determined by the customer. Versollan™ OM 1255NX-1 should not be left in the barrel for extended idle periods (greater than 5 minutes). Suggested Dewpoint: -40°F Injection Speed: 1 to 5 in/sec 1st Stage - Boost Pressure: 200 to 800 psi 2nd Stage - Hold Pressure: 70% of Boost Hold Time (Thick Part): 4 to 10 sec Hold Time (Thin Part): 1 to 3 sec

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.05 g/cc1.05 g/ccASTM D792
Viscosity 16700 cP
@Shear Rate 11200 1/s,
Temperature 200 °C
16700 cP
@Shear Rate 11200 1/s,
Temperature 392 °F
ASTM D3835
Maximum Moisture Content 0.020 - 0.0300.020 - 0.030
Linear Mold Shrinkage, Flow 0.0070 - 0.013 cm/cm0.0070 - 0.013 in/inASTM D955
Melt Flow  8.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
8.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 130 g/10 min
@Load 5.00 kg,
Temperature 200 °C
130 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 595910 sec; ASTM D2240
Tensile Strength at Break 6.58 MPa
@Temperature 23.0 °C
954 psi
@Temperature 73.4 °F
Die C2 hr; ASTM D412
Tensile Stress at Strain  1.93 MPa
@Strain 100 %,
Temperature 23.0 °C
280 psi
@Strain 100 %,
Temperature 73.4 °F
Die C2 hr; ASTM D412
 3.39 MPa
@Strain 300 %,
Temperature 23.0 °C
492 psi
@Strain 300 %,
Temperature 73.4 °F
Die C2 hr; ASTM D412
Elongation at Break 650 %
@Temperature 23.0 °C
650 %
@Temperature 73.4 °F
Die C2 hr; ASTM D412
Tear Strength 38.5 kN/m220 pliASTM D624
Compression Set 26 %
@Temperature 23.0 °C,
Time 79200 sec
26 %
@Temperature 73.4 °F,
Time 22.0 hour
ASTM D395B
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -68.5 °C-91.3 °FThickness = 1.90mm Conditioned for 40hrs at 23C at 50% RH; ASTM D746
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
UL 94
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 163 - 185 °C325 - 365 °F
Middle Barrel Temperature 168 - 196 °C334 - 385 °F
Front Barrel Temperature 177 - 210 °C351 - 410 °F
Nozzle Temperature 177 - 210 °C351 - 410 °F
Mold Temperature 21.1 - 48.9 °C70.0 - 120 °F
Drying Temperature 51.7 - 54.4 °C125 - 130 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour
Back Pressure 0.172 - 0.345 MPa24.9 - 50.0 psi
Screw Speed 75 - 125 rpm75 - 125 rpm
 
Descriptive Properties
Agency RatingsUL 94 .QMFZ2.E76261
AppearanceNatural Color
FeaturesGood Colorability
 Good Moldability
 Good Processability
 Low Gloss
FormsPellets
Generic MaterialTPE
Generic NameThermoplastic Elastomer (TPE)
Processing MethodInjection Molding
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
RoHS ComplianceRoHS Compliant
Suggested Max Regrind20%
UsesBusiness Equipment
 Consumer Applications
 Electrical/Electronic Applications
 Flexible Grips
 Overmolding
 Power/Other Tools
 Thin-walled Parts

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Avient Versollan™ OM 1255NX-9 Thermoplastic Elastomer (TPE)
Avient Versaflex™ OM 1245X-1 Thermoplastic Elastomer (TPE)
Avient Versollan™ OM 1262NX-1 Thermoplastic Elastomer (TPE)
Avient Versaflex™ OM 3060-1 Thermoplastic Elastomer (TPE)
LG Chemical MP211 ABS, Low Gloss, Metal Plating

PH0POL1212 / 145781

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.