MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Geon® Performance Solutions SF M7020 Polyvinyl Chloride, Rigid
Categories: Polymer; Thermoplastic; Vinyl (PVC); PVC, Rigid Grade

Material Notes:

Geon Performance Solutions was created from PolyOne in 2019.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.33 g/cc1.33 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0020 - 0.0050 cm/cm0.0020 - 0.0050 in/inASTM D955
Spiral Flow 119.38 cm47.000 in
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 7979ASTM D2240
Tensile Strength, Yield 41.4 MPa6000 psiType I, 51 mm/min; ASTM D638
Elongation at Break 35 %35 %Type I, 51 mm/min; ASTM D638
Tensile Modulus 2.28 GPa331 ksiType I, 51 mm/min; ASTM D638
Flexural Strength 62.7 MPa9090 psiASTM D790
Flexural Modulus 2.31 GPa335 ksiASTM D790
Izod Impact, Notched  1.10 J/cm
@Thickness 3.18 mm,
Temperature -18.0 °C
2.06 ft-lb/in
@Thickness 0.125 in,
Temperature -0.400 °F
Injection Molded; ASTM D256A
 2.70 J/cm
@Thickness 3.18 mm,
Temperature 0.000 °C
5.06 ft-lb/in
@Thickness 0.125 in,
Temperature 32.0 °F
Injection Molded; ASTM D256A
 6.40 J/cm
@Thickness 3.18 mm,
Temperature 23.0 °C
12.0 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
Injection Molded; ASTM D256A
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi)  67.2 °C
@Thickness 3.18 mm
153 °F
@Thickness 0.125 in
Unannealed; ASTM D648
 71.1 °C
@Thickness 3.18 mm
160 °F
@Thickness 0.125 in
Annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)  60.0 °C
@Thickness 3.18 mm
140 °F
@Thickness 0.125 in
Unannealed; ASTM D648
 70.0 °C
@Thickness 3.18 mm
158 °F
@Thickness 0.125 in
Annealed; ASTM D648
UL RTI, Electrical 90.0 °C194 °FUL 746
UL RTI, Mechanical with Impact 85.0 °C185 °FUL 746
UL RTI, Mechanical without Impact 90.0 °C194 °FUL 746
Flammability, UL94 V-0V-0
 5VA5VA
 V-0
@Thickness 1.80 mm
V-0
@Thickness 0.0709 in
ALL; UL 94
 5VA
@Thickness 1.80 mm
5VA
@Thickness 0.0709 in
ALL; UL 94
 5VA
@Thickness 1.60 mm
5VA
@Thickness 0.0630 in
All Colors
 
Processing PropertiesMetricEnglishComments
Melt Temperature 199 - 210 °C390 - 410 °F
 
Descriptive Properties
FeaturesGeneral Purpose
 High Flow
 High Impact Resistance
FormsPellets
Generic MaterialPVC, Rigid
Generic NamePolyvinyl Chloride, Rigid (PVC, Rigid)
Processing MethodInjection Molding
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
RoHS ComplianceRoHS Compliant
UsesMedical Appliances

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Colorite Polymers 2019F Rigid PVC
AlphaGary Dural 202/3 CLEAR 0003 Full Rigid Polyvinyl Chloride Compound
Geon® Performance Solutions HC 8210 Polyvinyl Chloride, Rigid
Fainplast Compounds MRT 256/G Medical Rigid PVC, Injection Molding
Fainplast Compounds MRT 168 Medical Rigid PVC, Injection Molding

PH0POL1279 / 145848

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.