MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Master Bond EP21TDC-2AN Two Component, Flexibilized, Highly Thermally Conductive, Electrically Insulating Epoxy Resin
Categories: Polymer; Thermoset; Epoxy; Epoxy Encapsulant, Unreinforced

Material Notes: Product Description: Master Bond Polymer System EP21TDC-2AN is a two component flexible epoxy resin compound for high performance bonding, sealing, coating, and encapsulation. This system’s thermal conductivity is formulated to fully cure at ambient temperature or more quickly at elevated temperatures with an easy to handle one to three mixing ratio by weight. The cured compound exhibits a high elongation (greater than 25%); good for a thermally conductive epoxy. After mixing EP21TDC-2AN generates a very low exotherm, which allows for a long working life. This epoxy compound exhibits good tensile shear and peel strength for bonding and sealing. It adheres well to a wide variety of substrates including metals, glass, ceramics, rubbers and many plastics. This cured adhesive is an excellent electrical insulator with superior chemical resistance to water, fuels and many solvents. It excels at withstanding thermal shock, thermal cycling and mechanical shock. This compound features a service temperature range of 4K to 250°F and has been successfully employed in a number of cryogenic applications. Master Bond EP21TDC-2AN is a versatile system that offers the structural benefits of an epoxy, yet incorporates flexibility and thermal conductivity. It is widely used in the electronic, electro-optical and related industries. The color of Part A is light gray; Part B is gray.

Product Advantages:

  • Convenient mixing: non-critical one to three mix ratio by weight
  • Easy application: product spreads evenly and smoothly.
  • Desirably long working life.
  • Versatile cure schedules: ambient temperature cures or fast elevated temperature cures.
  • High thermal conductivity combined with good electrical insulation properties.
  • High peel strength and elongation.
  • Excellent flexibility; exceptional thermal shock and chemical resistance.
  • Good bonding properties to similar and dissimilar substrates; superb impact resistance.
  • Cryogenically serviceable down to 4K.

Information provided by MasterBond®

Vendors: Master Bond is a leading manufacturer of adhesives, sealants, coatings and potting compounds. Master Bond’s vast product line consists of over 3,000 epoxy, polyurethane, silicone, cyanoacrylate and latex adhesives that vary in viscosity, cure speed, strength, chemical resistance, electrical properties, etc. Our custom adhesives offer design flexibility and provide excellent bonding performance. Visit www.masterbond.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Viscosity 45000 - 100000 cP45000 - 100000 cPPart A
 300000 - 700000 cP300000 - 700000 cPPart B
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 30 - 4030 - 40
Tensile Strength at Break >= 20.7 MPa
@Temperature 23.9 °C
>= 3000 psi
@Temperature 75.0 °F
Shear Strength >= 5.52 MPa>= 800 psiAl/Al, Tensile
Peel Strength >= 2.63 kN/m>= 15.0 pliT-peel
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+14 ohm-cm>= 1.00e+14 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 80.0 - 90.0 µm/m-°C44.4 - 50.0 µin/in-°F
Thermal Conductivity 3.17 - 3.46 W/m-K22.0 - 24.0 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 121 °C250 °F
Minimum Service Temperature, Air -269 °C-452 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  120 - 180 min
@Temperature 93.3 °C
2.00 - 3.00 hour
@Temperature 200 °F
 2880 - 4320 min
@Temperature 23.9 °C
48.0 - 72.0 hour
@Temperature 75.0 °F
Pot Life >= 60 min>= 60 min100 gram mass
Shelf Life 6.00 Month
@Temperature 23.9 °C
6.00 Month
@Temperature 75.0 °F
in original unopened containers
 
Descriptive Properties
Mixing Ratio (A to B)1:3by weight

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Master Bond EP21AOLV-2LO Two Part, Thermally Conductive and Electrically Insulative Epoxy
Master Bond EP21NDFG Two component epoxy compound for high performance applications
Master Bond EP21SC-1 Two Component Epoxy Resin System
Master Bond EP21TDCAOHT Two Component Thermally Conductive, Electrically Insulative Epoxy Adhesive
Master Bond EP42HT-2AO Two Component, Thermally Conductive, Heat Resistant Epoxy

PMASTB317 / 149564

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.