Celanese FORTRON 1120L4 PPS, 20% Specialty
Categories:
Polymer
;
Thermoplastic
;
Polyphenylene Sulfide (PPS)
;
Polyphenylene Sulfide (PPS) with 20% Glass Fiber Filler
Material Notes:
Fortron 1120L4 is a 20% glass fiber reinforced injection molding grade exhibiting excellent heat and chemical resistance, inherent flame retardancy, high hardness and stiffness at elevated temperatures.
Information provided by Celanese
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.47
g/cc
1.47
g/cc
ASTM D792
Density
1.48
g/cc
0.0535
lb/in³
ISO 1183
Water Absorption
0.030 %
@Temperature -17.8 °C
0.030 %
@Temperature 0.000 °F
24hr immersion; ASTM D570
Water Absorption at Saturation
0.020 %
0.020 %
ISO 62
Linear Mold Shrinkage, Flow
0.0030
-
0.0060
cm/cm
0.0030
-
0.0060
in/in
ISO 294-4
Linear Mold Shrinkage, Transverse
0.0070
-
0.010
cm/cm
0.0070
-
0.010
in/in
ISO 294-4
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell M
100
100
ISO 2039-2
102
102
ASTM D785
Tensile Strength at Break
120
MPa
17400
psi
5mm/min; ISO 527-2/1A
126
MPa
18300
psi
ASTM D638
Elongation at Break
1.5 %
1.5 %
5mm/min; ISO 527-2/1A
1.8 %
1.8 %
ASTM D638
Flexural Strength
170
MPa
24700
psi
ISO 178
177.5
MPa
25750
psi
ASTM D790
Flexural Modulus
7.52
GPa
1090
ksi
ASTM D790
8.00
GPa
1160
ksi
ISO 178
Izod Impact, Notched
0.587
J/cm
1.10
ft-lb/in
ASTM D256
Izod Impact, Notched (ISO)
7.00
kJ/m²
3.33
ft-lb/in²
ISO 180/1A
35.0
kJ/m²
@Temperature 23.0 °C
16.7
ft-lb/in²
@Temperature 73.4 °F
ISO 180/1U
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
26.0
µm/m-°C
14.4
µin/in-°F
ISO 11359-2
CTE, linear, Transverse to Flow
53.0
µm/m-°C
29.4
µin/in-°F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)
280
°C
536
°F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
255
°C
491
°F
ISO 75-1, -2
260
°C
500
°F
ASTM D648
Flammability, UL94
V-0
V-0
V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
Processing Properties
Metric
English
Comments
Processing Temperature
140
-
160
°C
284
-
320
°F
cavity
330
-
340
°C
626
-
644
°F
hot runner
Feed Temperature
60.0
-
80.0
°C
140
-
176
°F
Zone 1
290
-
300
°C
554
-
572
°F
Zone 2
310
-
320
°C
590
-
608
°F
Zone 3
330
-
340
°C
626
-
644
°F
Zone 4
330
-
340
°C
626
-
644
°F
Die Temperature
310
-
330
°C
590
-
626
°F
Melt Temperature
330
-
340
°C
626
-
644
°F
Drying Temperature
130
-
140
°C
266
-
284
°F
Dry Time
3.00
-
4.00
hour
3.00
-
4.00
hour
Moisture Content
<= 0.020 %
<= 0.020 %
Injection Pressure
50.0
-
100
MPa
7250
-
14500
psi
Hold Pressure
30.0
-
70.0
MPa
4350
-
10200
psi
Back Pressure
<=
3.00
MPa
<=
435
psi
Screw Speed
50
rpm
@Diameter 55.0 mm
50
rpm
@Diameter 2.17 in
75
rpm
@Diameter 40.0 mm
75
rpm
@Diameter 1.57 in
120
rpm
@Diameter 25.0 mm
120
rpm
@Diameter 0.984 in
Descriptive Properties
Injection speed
fast
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Celanese FORTRON 205 PPS, Unfilled
Celanese FORTRON 1130L4 PPS, 30% Glass Reinforced
Celanese FORTRON 320 PPS, Unfilled
Celanese Rynite® FR530 BK507 PET-GF30FR(17)
Celanese FORTRON 1140L0 PPS, 40% Glass Reinforced
PHCQ265 / 178720
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.