MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Alcoa 2324-T39 Aluminum Plate
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Alloy 2324-T39 is a higher strength version of alloy 2024-T351 and is a purity controlled composition variant of alloy 2024. It was developed for tension-dominated, fatigue and fracture critical plate applications. The T39 temper, developed through special fabricating practices, improves both strength and fracture toughness properties over alloy 2024 plate. Alloy 2324-T39 plate is being used successfully on lower wing skin and center wing box components of commercial aircraft.

Information provided by Alcoa.

Key Words: Aluminium
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.77 g/cc0.100 lb/in³per Aluminum Association
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate >= 475 MPa>= 68900 psiGuaranteed minimum; long transverse
Tensile Strength, Yield >= 370 MPa>= 53700 psiGuaranteed minimum; long transverse
Elongation at Break >= 8.0 %>= 8.0 %Guaranteed minimum; long transverse
Modulus of Elasticity 72.4 GPa10500 ksiAA2024
Poissons Ratio 0.330.33AA2024
Shear Modulus 27.0 GPa3920 ksiAA2024
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000449 ohm-cm0.00000449 ohm-cmAA2024
 
Thermal PropertiesMetricEnglishComments
CTE, linear  23.2 µm/m-°C
@Temperature 20.0 °C
12.9 µin/in-°F
@Temperature 68.0 °F
AA2024
 24.7 µm/m-°C
@Temperature 20.0 - 300 °C
13.7 µin/in-°F
@Temperature 68.0 - 572 °F
average; AA2024
Specific Heat Capacity 0.875 J/g-°C0.209 BTU/lb-°FAA2024
Thermal Conductivity 151 W/m-K1050 BTU-in/hr-ft²-°FAA2024
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 92 - 94.7 %92 - 94.7 %As Remainder
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu 3.8 - 4.4 %3.8 - 4.4 %
Iron, Fe <= 0.12 %<= 0.12 %
Magnesium, Mg 1.2 - 1.8 %1.2 - 1.8 %
Manganese, Mn 0.30 - 0.90 %0.30 - 0.90 %
Other, each <= 0.050 %<= 0.050 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.10 %<= 0.10 %
Titanium, Ti <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.25 %<= 0.25 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2324-T39
Alcoa 7055-T7751 Aluminum Plate
Aluminum 2024-T4; 2024-T351
Alpase K100-S™ Aluminum Plate
Aluminum 6063-T1

NALCOA40 / 14755

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.