MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

A. Schulman Diamond ABSPC 9901GF20 Injection Molding Grade, 20% Glass Filled
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Glass Fiber Filled; Polycarbonate (PC)

Material Notes:

A. Schulman has acquired Network Polymers & Diamond Polymers.

Key Words: Acrylonitrile Butadiene Styrene, Polycarbonate
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.27 g/cc1.27 g/ccASTM D792
Melt Flow 22 g/10 min
@Load 5.00 kg,
Temperature 265 °C
22 g/10 min
@Load 11.0 lb,
Temperature 509 °F
ASTM D1238
Ash 18 - 22 %18 - 22 %ASTM D5630
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 74.1 MPa10700 psichs 2.0 in/min; ASTM D638
Elongation at Break 1.9 %1.9 %chs 2.0 in/min; ASTM D638
Flexural Strength 109.6 MPa
@Thickness 3.17 mm
15900 psi
@Thickness 0.125 in
chs 0.05 in/min; ASTM D790
Flexural Modulus 4.823 GPa
@Thickness 3.17 mm
699.5 ksi
@Thickness 0.125 in
tangent; chs 0.05 in/min; ASTM D790
Izod Impact, Notched 0.801 J/cm
@Thickness 3.17 mm,
Temperature 23.0 °C
1.50 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 137 °C
@Load 1.00 kg,
Thickness 3.17 mm
279 °F
@Load 2.20 lb,
Thickness 0.125 in
ASTM D1525

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Cossa Polimeri ESTABLEND 0840 GF Polycarbonate ABS Blend, 20% Glass Filled
Cossa Polimeri ESTABLEND 0820 GF Polycarbonate ABS Blend, 10% Glass Filled
LATI LASTILAC 11 G/20-V0 20% Glass Fiber Reinforced ABS/PC-Based Alloy
Covestro Bayblend® FR 3310 TV PC/ABS Blend, 15% Glass Reinforced
Kingfa JH-R2G10 P60 10% Glass Fiber Reinforced PC/ABS Alloy

PDIAM337 / 126428

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.