MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ATI Allegheny Ludlum Stainless Steel 334 (UNS S33400)  (discontinued **)
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Allegheny Ludlum Type 334 is a titanium- and aluminum-bearing austenitic stainless steel offering superior elevated temperature scaling resistance compared to the conventional chromium-nickel stainless steels such as Type 304. The oxidation resistance of Type 334 compares favorably with higher alloyed grades up to 1900°F, making it a good candidate alloy for use in emission control systems, and other applications where resistance to elevated temperature degradation is important.

Information provided by Allegheny Ludlum Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.03 g/cc0.290 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 8282
Tensile Strength, Ultimate 572.4 MPa83020 psi
 103.4 MPa
@Temperature 982 °C
15000 psi
@Temperature 1800 °F
1800°F
 469 MPa
@Temperature 538 °C
68000 psi
@Temperature 1000 °F
1000°F
Tensile Strength, Yield 241.4 MPa35010 psi
 62.8 MPa
@Temperature 982 °C
9110 psi
@Temperature 1800 °F
 172.4 MPa
@Temperature 538 °C
25000 psi
@Temperature 1000 °F
Elongation at Break 40 %40 %
Modulus of Elasticity 200 GPa29000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000891 ohm-cm0.0000891 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  17.04 µm/m-°C
@Temperature 20.0 - 100 °C
9.467 µin/in-°F
@Temperature 68.0 - 212 °F
 17.48 µm/m-°C
@Temperature 20.0 - 200 °C
9.711 µin/in-°F
@Temperature 68.0 - 392 °F
 17.66 µm/m-°C
@Temperature 20.0 - 250 °C
9.811 µin/in-°F
@Temperature 68.0 - 482 °F
 18.31 µm/m-°C
@Temperature 20.0 - 400 °C
10.17 µin/in-°F
@Temperature 68.0 - 752 °F
 18.54 µm/m-°C
@Temperature 20.0 - 500 °C
10.30 µin/in-°F
@Temperature 68.0 - 932 °F
 19.22 µm/m-°C
@Temperature 20.0 - 700 °C
10.68 µin/in-°F
@Temperature 68.0 - 1290 °F
Thermal Conductivity 12.9 W/m-K
@Temperature 20.0 - 50.0 °C
89.5 BTU-in/hr-ft²-°F
@Temperature 68.0 - 122 °F
Maximum Service Temperature, Air 1038 °C1900 °Foxidation resistance is good
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.40 %<= 0.40 %
Carbon, C <= 0.030 %<= 0.030 %
Chromium, Cr 19 - 19.5 %19 - 19.5 %
Copper, Cu <= 0.20 %<= 0.20 %
Iron, Fe 60 %60 %as balance
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni 19 - 20 %19 - 20 %
Phosphorus, P <= 0.020 %<= 0.020 %
Silicon, Si <= 0.75 %<= 0.75 %
Sulfur, S <= 0.015 %<= 0.015 %
Titanium, Ti <= 0.40 %<= 0.40 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Haynes 188 alloy, 0% cold reduction, 3.2 mm thick sheet
Haynes Hastelloy® S alloy, flat products
309 Stainless Steel, annealed, sheet
Outokumpu 153MA™ High Temperature Austenitic Stainless Steel
Overview of materials for Austenitic

NL334 / 17883

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.