MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

EMS-Grivory Grilamid® L 20 H FR PA12 FR
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12); Nylon 12, Flame Retardant

Material Notes: Product Description: Grilamid L 20 H FR is a flame retarded, medium viscosity product, based on Polyamide 12 (PA12). Grilamid L 20 H FR contains no halogen or phosphorus, it has a light natural color and is heat stabilized. Grilamid L 20 H FR is used for production of high value injection molding and extrusion parts. The special features of Grilamid L 20 H FR are:
  • Flame resistant, UL94 V-2 at 0.8 mm
  • Halogen and phosphorus free
  • Light natural color
  • Glow wire temperature 960°C at 1mm
  • Heat stability
  • Good chemical resistance
  • High surface quality
  • Good dimensional stability
  • High processing speed
  • Low density, low weight
Application examples: Grilamid L 20 H FR is suitable for injection molding and extrusion parts in electro/electronic applications.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³Dry; ISO 1183
Water Absorption 1.4 %1.4 %Sim. to ISO 62
Moisture Absorption 0.700 %0.700 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0060 cm/cm0.0060 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 72
@Time 15.0 sec
72
@Time 0.00417 hour
Conditioned; ISO 868
Tensile Strength at Break 35.0 MPa5080 psiConditioned; ISO 527-1/-2
 40.0 MPa5800 psiDry; ISO 527-1/-2
Tensile Strength, Yield 40.0 MPa5800 psiConditioned; ISO 527-1/-2
 50.0 MPa7250 psiDry; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Nominal, Dry; ISO 527-1/-2
 >= 50 %>= 50 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 5.0 %5.0 %Dry; ISO 527-1/-2
 10 %10 %Conditioned; ISO 527-1/-2
Tensile Modulus 1.50 GPa218 ksiConditioned; ISO 527-1/-2
 1.90 GPa276 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 0.700 J/cm²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+12 ohm-cm1.00e+12 ohm-cmConditioned; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmIEC 60093
Dielectric Strength 34.0 kV/mm864 kV/inConditioned; IEC 60243-1
Comparative Tracking Index 600 V600 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 90.0 µm/m-°C50.0 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 120 µm/m-°C66.7 µin/in-°FISO 11359-1/-2
Melting Point 178 °C352 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 90.0 - 110 °C194 - 230 °FLong Term; ISO 2578
 150 °C302 °FShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 130 °C266 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 50.0 °C122 °FISO 75-1/-2
Flammability, UL94 V-2V-2IEC 60695-11-10
 
Descriptive Properties
AutomotiveAutomotive electr. and electronics, lighting
Electricals & ElectronicsCables & Tubes
 Connectors
 Energy distribution
FormGranules
ProcessingOther Extrusion
Special CharacteristicsFlame retardant
 Improved heat resistance
 Improved UV resistance (outdoor use)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Arkema Rilsamid® AESN BLACK P202 T6L PA12-I
Celanese Zytel® FR7026V0F NC010 PA66-FR(30)
EMS-Grivory Grilon® BG-30 FR PA6-GF30 FR
RTP Company RTP 299 F X 125585 H Nylon 12 (PA); Flame Retardant - Halogen Free
Celanese Zytel® HTNFR52G30BL BK337 PA6T/66-GF30FR(16+72)

PGRH028 / 156737

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.