MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Baystar™ 2285 HDPE Bimodal Film Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Film Grade

Material Notes: Characteristics:

  • Bimodal molecular weight distribution
  • Excellent tear strength
  • Exceptional impact strength
  • Excellent processability

Applications:

  • T-shirt sacks
  • Trash can liners
  • Merchandise bags
  • Multi-wall liners
  • Deli wrap

Film tested was produced at 0.8 mil with a 4:1 BUR.

This former Total Petrochemicals grade is now a part of the Bayport Polymers joint venture.

Key Words: Excellent Tear Strength, Impact Strength, and Processability
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.951 g/cc0.0344 lb/in³ASTM D-792
Melt Flow  0.080 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.080 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D-1238
 0.32 g/10 min
@Load 5.00 kg,
Temperature 190 °C
0.32 g/10 min
@Load 11.0 lb,
Temperature 374 °F
ASTM D-1238
High Load Melt Index 11 g/10 min
@Load 21.6 kg,
Temperature 190 °C
11 g/10 min
@Load 47.6 lb,
Temperature 374 °F
ASTM D-1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 36.5 MPa5300 psiASTM D-882, A
Film Tensile Strength at Yield, TD 34.5 MPa5000 psiASTM D-882, A
Film Elongation at Break, MD 400 %400 %ASTM D-882, A
Film Elongation at Break, TD 400 %400 %ASTM D-882, A
Elmendorf Tear Strength MD 24 g24 gASTM D-1922
Elmendorf Tear Strength TD 120 g120 gASTM D-1922
Dart Drop Test 350 g0.772 lbASTM D-1709, A
Film Tensile Strength at Break, MD 63.4 MPa9200 psiASTM D-882, A
Film Tensile Strength at Break, TD 67.6 MPa9800 psiASTM D-882, A
1% Secant Modulus, MD 841 MPa122000 psiASTM D-882, A
1% Secant Modulus, TD 910 MPa132000 psiASTM D-882, A
 
Thermal PropertiesMetricEnglishComments
Melting Point 132 °C270 °FASTM D3417
 
Descriptive Properties
processFilm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Borealis FS1560 High Density Polyethylene
Formosa Plastics Formolene® E927 Film HDPE
Iran Petrochemical (PCC) EX 5 HM 9450 F High Density Polyethylene
Borealis CG9620 High Density Polyethylene
ExxonMobil HD 6001 High Density Polyethylene (HDPE), Film Grade

PBAYST800 / 38670

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.