MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Hanwha Azdel Plus U421-B01 42% Directionalized Continuous Fiber Mat / PP Resin Matrix
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: AZDEL® U421-B01 is a glass mat thermoplastic laminate based upon a combination of random oriented continuous fiber mat and oriented fiber mat contained within a polypropylene resin matrix. This composite material exhibits highly oriented material properties in the longitudinal direction of the oriented glass fibers. This material is typically used in semi-structural applications where high material properties in one direction are desired, such as automotive bumper beams.

Mechanical properties and mold shrinkage measured on flat plaques.

Information provided by Azdel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.21 g/cc1.21 g/ccLaminate; ASTM D792
 1.24 g/cc1.24 g/ccMolded; ASTM D792
Filler Content 42 %42 %By weight (ashing); Internal
Thickness 3900 microns154 milSheet; Internal
Linear Mold Shrinkage 0.0010 - 0.0030 cm/cm0.0010 - 0.0030 in/inMeasured on flat plaques; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 60.0 MPa8700 psiTransverse direction; ISO 527
 276 MPa40000 psiLongitudinal direction; ISO 527
Elongation at Break 2.3 %2.3 %Transverse direction; ISO 527
 2.5 %2.5 %Longitudinal direction; ISO 527
Tensile Modulus 5.31 GPa770 ksiTransverse direction; ISO 527
 10.1 GPa1460 ksiLongitudinal direction; ISO 527
Flexural Strength 145 MPa21000 psiTransverse direction; ISO 178
 260 MPa37700 psiLongitudinal direction; ISO 178
Flexural Modulus 4.80 GPa696 ksiTransverse direction; ISO 178
 7.69 GPa1120 ksiLongitudinal direction; ISO 178
Poissons Ratio 0.3610.361Transverse direction; ISO 527
 0.3770.377Longitudinal direction; ISO 527
Izod Impact, Notched  7.20 J/cm
@Thickness 4.00 mm,
Temperature 23.0 °C
13.5 ft-lb/in
@Thickness 0.157 in,
Temperature 73.4 °F
transverse direction; ISO 180
 16.5 J/cm
@Thickness 4.00 mm,
Temperature 23.0 °C
30.9 ft-lb/in
@Thickness 0.157 in,
Temperature 73.4 °F
longitudinal direction; ISO 180
Impact 700
@Thickness 4.00 mm
700
@Thickness 0.157 in
Multi-axial in kg, at max. load; ASTM D3763
Impact Test  38.0 J
@Thickness 4.00 mm
28.0 ft-lb
@Thickness 0.157 in
Multi-axial, at max. load; ASTM D3763
 58.0 J
@Thickness 4.00 mm
42.8 ft-lb
@Thickness 0.157 in
Multi-axial, at failure; ASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear 37.0 µm/m-°C
@Temperature -40.0 - 120 °C
20.6 µin/in-°F
@Temperature -40.0 - 248 °F
longitudinal direction; ASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 143 °C289 °FTransverse direction; ASTM D648
 158 °C316 °FLongitudinal direction; ASTM D648
Flame Spread 4.57 mm/min0.180 in/minlongitudinal direction; FMVSS302
 4.57 mm/min0.180 in/mintransverse direction; FMVSS302
 
Descriptive Properties
ColorBlackInternal

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Hanwha Azdel Plus R401-B01 40% Continuous Random Fiber Mat / PP Resin Matrix
Hanwha Azdel Plus R300-B01 30% Continuous Random Fiber Mat / PP Resin Matrix
Hanwha Azdel Plus C200B01N 20% Chopped Fiber Mat / PP Resin Matrix
Hanwha Azdel AZMET® CM32350 35% continuous random fiber mat / PET resin matrix
Hanwha Azdel AZMET® CM20350 35% continuous random fiber mat / PBT resin matrix

PZZGEAZ71 / 40620

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.