MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Avient Therma-Tech™ SF-4500 TC Polyphenylene Sulfide (PPS)
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS)

Material Notes:

Information provided by PolyOne

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.67 g/cc1.67 g/ccASTM D792
Water Absorption 0.040 %0.040 %@ 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0010 cm/cm0.0010 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 123123ASTM D785
Tensile Strength at Break 100 MPa14500 psiType I, 5.1 mm/min; ASTM D638
Elongation at Break 2.0 %2.0 %Type I, 5.1 mm/min; ASTM D638
Tensile Modulus 31.0 GPa4500 ksiType I, 5.1 mm/min; ASTM D638
Flexural Strength 296 MPa42900 psiASTM D790
Flexural Modulus 20.0 GPa2900 ksiASTM D790
Compressive Strength 193 MPa28000 psiASTM D695
Izod Impact, Notched 0.170 J/cm
@Thickness 3.18 mm,
Temperature 23.0 °C
0.318 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
Injection Molded; ASTM D256A
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 80 - 100 ohm-cm80 - 100 ohm-cmASTM D257
Surface Resistance 80 - 100 ohm80 - 100 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 11.0 µm/m-°C6.11 µin/in-°FASTM D696
Thermal Conductivity 11.0 W/m-K76.3 BTU-in/hr-ft²-°FASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 299 °C
@Thickness 3.18 mm
570 °F
@Thickness 0.125 in
Annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 263 °C
@Thickness 3.18 mm
505 °F
@Thickness 0.125 in
Annealed; ASTM D648
Flammability, UL94 V-0V-0UL 94
 
Processing PropertiesMetricEnglishComments
Melt Temperature 304 - 332 °C579 - 630 °F
Mold Temperature 121 - 149 °C250 - 300 °F
Drying Temperature 149 °C300 °F
Dry Time 6.00 hour6.00 hour
 
Descriptive Properties
FeaturesElectrically Conductive
 Thermally Conductive
FormsPellets
Generic MaterialPPS
Generic NamePolyphenylene Sulfide (PPS)
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Avient Therma-Tech™ LC-6000 TC Liquid Crystal Polymer (LCP)
LATI Laticonther 80 GR/50 PPS, 50% Graphite Reinforced
Avient Therma-Tech™ NJ-6000 TC Polyamide 12 (Nylon 12)
Avient Therma-Tech™ SF-5000C TC Polyphenylene Sulfide (PPS)
Avient Therma-Tech™ SF-6000 TC Polyphenylene Sulfide (PPS)

PH0POL0185 / 144754

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.