MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Industeel CLC 17.13.3 LN Nitrogen Containing 18Cr-10Ni-2Mo Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel; T S30000 Series Stainless Steel

Material Notes: Description: CLC 17-13-3LN is a nitrogen alloyed austenitic stainless steel with Mo additions. Its low carbon content avoids intergranular corrosion, even on welded pieces without an ulterior water quenching. Alloys CLC 17-13-3LN exhibits austenitic microstructure free of deleterious carbide precipitations in grain boundaries. The grade contains residual ferrite (= 2%) after solution annealing (1050 - 1150°C / 1922 - 2102°F) and water quenching. Higher Molybdenum content improves uniform and localized corrosion resistance. Nitrogen additions improve the structure stability and increase the yield strength compared to CLC 17-12-2L. Main properties of CLC 17-13-3LN are : high ductility, easy weldability, mirror polishability. Typical applications are food and beverage processing industry, chemical industry and chemical tankers.

Information provided by manufacturer.

Key Words: EURONORM 1.4429 X2CrNiMoN17.13.3, AFNOR Z3CND 17.12Az, DIN W 1.4429, ASTM A240 TP 316LN, UNS S31653
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.95 g/cc0.287 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 637 MPa92400 psiTypical
 580 - 780 MPa84100 - 113000 psiMinimum Guaranteed
Tensile Strength, Yield  >= 280 MPa
@Strain 0.2 %
>= 40600 psi
@Strain 0.2 %
 >= 320 MPa
@Strain 1 %
>= 46400 psi
@Strain 1 %
 355 MPa
@Strain 0.2 %
51500 psi
@Strain 0.2 %
Typical
Elongation at Break >= 45 %>= 45 %
 58 %58 %Typical
Creep Strength 270 MPa
@Temperature 600 °C,
Time 3.60e+6 sec
39200 psi
@Temperature 1110 °F,
Time 1000 hour
Modulus of Elasticity 200 GPa
@Temperature 20.0 - 100 °C
29000 ksi
@Temperature 68.0 - 212 °F
Poissons Ratio 0.2990.299Calculated
Shear Modulus 77.0 GPa
@Temperature 20.0 - 100 °C
11200 ksi
@Temperature 68.0 - 212 °F
Charpy Impact >= 187 J>= 138 ft-lb
 325 J240 ft-lbTypical
 >= 125 J
@Temperature -196 °C
>= 92.2 ft-lb
@Temperature -321 °F
 250 J
@Temperature -196 °C
184 ft-lb
@Temperature -321 °F
Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000750 ohm-cm
@Temperature 20.0 - 100 °C
0.0000750 ohm-cm
@Temperature 68.0 - 212 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.0 µm/m-°C
@Temperature 20.0 - 100 °C
8.89 µin/in-°F
@Temperature 68.0 - 212 °F
 16.5 µm/m-°C
@Temperature 20.0 - 200 °C
9.17 µin/in-°F
@Temperature 68.0 - 392 °F
 17.0 µm/m-°C
@Temperature 20.0 - 300 °C
9.44 µin/in-°F
@Temperature 68.0 - 572 °F
 18.0 µm/m-°C
@Temperature 20.0 - 500 °C
10.0 µin/in-°F
@Temperature 68.0 - 932 °F
Specific Heat Capacity 0.500 J/g-°C
@Temperature 20.0 - 100 °C
0.120 BTU/lb-°F
@Temperature 68.0 - 212 °F
Thermal Conductivity 15.0 W/m-K
@Temperature 20.0 - 100 °C
104 BTU-in/hr-ft²-°F
@Temperature 68.0 - 212 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.030 %0.030 %
Chromium, Cr 17.9 %17.9 %
Iron, Fe 68.51 %68.51 %As remainder
Molybdenum, Mo 2.6 %2.6 %
Nickel, Ni 10.8 %10.8 %
Nitrogen, N 0.16 %0.16 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 316LN Stainless Steel, Composition Spec
Outokumpu 4429 Cr-Ni-Mo Austenitic Stainless Steel
AISI 316N Cast Stainless Steel, UNS J92804
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 900 (Age-Hardened 482°C/1hr/AC)
Cast Stainless Steel CF3MN, ASTM A351

NINDUST08 / 17546

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.