MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Bakelite® EP 8412 Epoxy Resin, High Arc Resistance, Improved Electrical Properties, Low Shrinkage
Categories: Polymer; Thermoset; Epoxy; Epoxy Molding Compound; Filled/Reinforced Thermoset

Material Notes: Epoxy molding compound, inorganically filled, glass fiber reinforced, heat resistant, dimensionally stable, good electric and mechanical properties, very good chemical resistance, low viscosity, UL listed (RTI 155°C).

Applications: Encapsulation of electric parts, e. g. electromagnetic coil

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.89 g/cc0.0683 lb/in³ISO 1183
Apparent Bulk Density 0.850 g/cc0.0307 lb/in³ISO 60
Linear Mold Shrinkage 0.0025 cm/cm0.0025 in/inCompression Molding. Post Shrinkage = 0.01%.; ISO 2577
 0.0030 cm/cm0.0030 in/inInjection Molding. Post Shrinkage = 0.02%.; ISO 2577
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 400 MPa58000 psiH961/30; ISO 2039/P1
Tensile Strength 55.0 MPa7980 psiISO 527 - 1/2
Tensile Modulus 13.0 GPa1890 ksiISO 527 - 1/2
Flexural Strength 125 MPa18100 psiISO 178
Flexural Modulus 15.5 GPa2250 ksiISO 178
Compressive Strength 170 MPa24700 psiISO 604
Charpy Impact Unnotched 0.850 J/cm²4.04 ft-lb/in²ISO 179-1 eU
Charpy Impact, Notched 0.400 J/cm²1.90 ft-lb/in²ISO 179-1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cm
Surface Resistance 1.00e+12 ohm1.00e+12 ohm
Dielectric Constant 5.5
@Frequency 100 Hz
5.5
@Frequency 100 Hz
Dielectric Strength 30.0 kV/mm
@Thickness 1.00 mm
762 kV/in
@Thickness 0.0394 in
IEC 60243-P1
Dissipation Factor 0.020
@Frequency 100 Hz
0.020
@Frequency 100 Hz
Arc Resistance 192 - 194 sec192 - 194 secASTM D495
High Voltage Arc Resistance to Ignition (HVAR) >= 300 sec
@Thickness 1.50 mm
>= 300 sec
@Thickness 0.0591 in
BK
Comparative Tracking Index 250 V250 VIEC 6011
Hot Wire Ignition, HWI  60 - 120 sec
@Thickness 1.50 mm
60 - 120 sec
@Thickness 0.0591 in
BK
 >= 120 sec
@Thickness 3.00 mm
>= 120 sec
@Thickness 0.118 in
BK
High Amp Arc Ignition, HAI  15 - 30 arcs
@Thickness 1.50 mm
15 - 30 arcs
@Thickness 0.0591 in
BK
 60 - 120 arcs
@Thickness 3.00 mm
60 - 120 arcs
@Thickness 0.118 in
BK
High Voltage Arc-Tracking Rate, HVTR 0.000 - 10.0 mm/min
@Thickness 3.00 mm
0.000 - 0.394 in/min
@Thickness 0.118 in
BK
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 180 °C356 °F<20000 hours; IEC 60216-P1
 220 °C428 °F< 50 hours; IEC 60216-P1
Deflection Temperature at 8.0 MPa 120 °C248 °FISO 75-2
UL RTI, Electrical 155 °C
@Thickness 1.50 mm
311 °F
@Thickness 0.0591 in
BK
UL RTI, Mechanical with Impact 155 °C
@Thickness 1.50 mm
311 °F
@Thickness 0.0591 in
BK
UL RTI, Mechanical without Impact 155 °C
@Thickness 1.50 mm
311 °F
@Thickness 0.0591 in
BK
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
BK
 
Processing PropertiesMetricEnglishComments
Feed Temperature 60.0 - 75.0 °C140 - 167 °FInjection molding
Nozzle Temperature 70.0 - 100 °C158 - 212 °FInjection molding
Melt Temperature 90.0 - 100 °C194 - 212 °FInjection molding
Mold Temperature 160 - 190 °C320 - 374 °FCompression molding
 170 - 190 °C338 - 374 °FInjection molding
Injection Pressure >= 10.0 MPa>= 1450 psiCompression and injection cavity mold pressure
Back Pressure 0.500 - 2.00 MPa72.5 - 290 psiInjection molding
Cure Time 0.250 - 0.417 min0.00417 - 0.00694 hourPer 1 mm of wall thickness, injection molding
 0.500 - 1.00 min0.00833 - 0.0167 hourPer 1 mm of wall thickness, compression molding
 
Descriptive Properties
Chromatic SpectrumSubdued Colors
Creep Rupture StrengthVery Good
Holding PressureApproximately 40-60% of injection pressure
Media ResistanceVery Good
Thermal ExpansionVery Slight
Water absorption (mg)624h / 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bakelite® EP 8414 Epoxy Resin, High Arc Resistance, Improved Electrical Properties, Low Shrinkage
Huntsman Araldite GY 281 Bisphenol F Epoxy Resin
Bakelite® EP 8413 Epoxy Molding Compound
Solvay CYCOM® 7668 Epoxy Resin
Overview of materials for Polytetrafluoroethylene (PTFE), Molded

PBAKE000 / 27034

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.