MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Parson Adhesives PARTITE® 7405 Methacrylate Structural Adhesive
Categories: Polymer; Adhesive

Material Notes: PARTITE 7405 is a two-component, 100% reactive, toughened structural methacrylate adhesive specifically formulated for bonding wide variety of metals, thermoplastics, thermosets, and composite assemblies.

FEATURE:

  • Combined at a 10:1 mix ratio, Non-sagging and thixotropic formulation
  • Excellent impact, peel and shear resistance
  • Excellent low temperature properties.
  • Working time 8 to 12 minutes and achieves 80% ultimate strength in 15 minutes.
APPLICATIONS:
  • Ideal for bonding all types of PVC, Polycarbonate, Acrylic, Fiberglass, PBT, PPO, ABS, FRT, Polyurethane, Epoxy, Wood, RIM, Nylon, FRP, Polyesters, Gelcoats, Styrene, Stainless Steel, Carbon Steel, Galvanized Steel, etc.
  • Ideal for Automotive Components, transportation industry, Sporting goods, Electronics Parts, Tool handles, Appliances, Computer Assemblies, Electrical Components, Furniture, Marine assemblies, Plastic Fabrications, Sign & Display, Composite assemblies, etc.

Information provided by Parson Adhesives, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.959 g/cc0.0346 lb/in³Adhesive
 0.971 g/cc0.0351 lb/in³Mixed
 1.07 g/cc0.0387 lb/in³Activator
Brookfield Viscosity 50000 - 70000 cP50000 - 70000 cPRVT, Activator
 100000 - 125000 cP100000 - 125000 cPRVT, Adhesive
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 7373ASTM D2240
Elongation at Break 90 %90 %
Shear Strength >= 10.7 MPa>= 1550 psiFiberglass; ASTM D1002
 11.0 MPa1600 psiABS/PVC; ASTM D1002
 12.4 - 15.9 MPa1800 - 2300 psiDIN 53283
 >= 19.3 MPa>= 2800 psiAl/Al; ASTM D1002
 24.5 MPa3550 psiSteel/Steel; ASTM D1002
Tensile Impact 11.2 J/cm21.0 ft-lb/in
Peel Strength 2.80 - 3.86 kN/m16.0 - 22.0 pli
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 121 °C250 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
Flash Point 51.0 °C124 °FAdhesive
 51.0 °C124 °FActivator
 
Processing PropertiesMetricEnglishComments
Cure Time 25.0 - 30.0 min0.417 - 0.500 hourFixture Time
 60.0 - 180 min1.00 - 3.00 hourFunctional
 1440 min24.0 hourFull
Working Life 8.00 - 12.0 min8.00 - 12.0 min
 
Descriptive Properties
ColorMilky-WhiteAdhesive
 Off-WhiteActivator
Gap Filling<0.25 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Makroblend® UT305 PC/PET Blend
DuPont Mobility and Materials Rynite® FR530L BK507 Polyethylene Terephthalate (PET)
Devcon Wear Guard (High Load) Epoxy
Devcon Plastic Steel® Putty (A) Epoxy
DAK Americas Laser+® HS AD600A PET

PPARSN096 / 186539

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.