Physical Properties | Metric | English | Comments |
---|
Density | 7.845 g/cc | 0.2834 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 143 | 143 |
Hardness, Knoop | 163 | 163 |
Hardness, Rockwell B | 78 | 78 |
Hardness, Vickers | 149 | 149 |
Tensile Strength, Ultimate | 485 MPa | 70300 psi |
Tensile Strength, Yield | 450 MPa | 65300 psi |
Elongation at Break | 12 % | 12 % |
Reduction of Area | 35 % | 35 % |
Modulus of Elasticity | 200 GPa | 29000 ksi |
Bulk Modulus | 160 GPa | 23200 ksi |
Poissons Ratio | 0.29 | 0.29 |
Shear Modulus | 80.0 GPa | 11600 ksi |
Izod Impact | 45.0 J | 33.2 ft-lb |
| 49.0 J | 36.1 ft-lb |
| 65.0 J | 47.9 ft-lb |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000171 ohm-cm @Temperature 20.0 °C | 0.0000171 ohm-cm @Temperature 68.0 °F |
| 0.0000221 ohm-cm @Temperature 100 °C | 0.0000221 ohm-cm @Temperature 212 °F |
| 0.0000296 ohm-cm @Temperature 200 °C | 0.0000296 ohm-cm @Temperature 392 °F |
| 0.0000493 ohm-cm @Temperature 400 °C | 0.0000493 ohm-cm @Temperature 752 °F |
| 0.0000763 ohm-cm @Temperature 600 °C | 0.0000763 ohm-cm @Temperature 1110 °F |
| 0.0000932 ohm-cm @Temperature 700 °C | 0.0000932 ohm-cm @Temperature 1290 °F |
| 0.0001111 ohm-cm @Temperature 800 °C | 0.0001111 ohm-cm @Temperature 1470 °F |
| 0.0001149 ohm-cm @Temperature 900 °C | 0.0001149 ohm-cm @Temperature 1650 °F |
| 0.0001179 ohm-cm @Temperature 1000 °C | 0.0001179 ohm-cm @Temperature 1830 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 11.3 µm/m-°C @Temperature 20.0 - 100 °C | 6.28 µin/in-°F @Temperature 68.0 - 212 °F |
| 12.1 µm/m-°C @Temperature 20.0 - 200 °C | 6.72 µin/in-°F @Temperature 68.0 - 392 °F |
| 12.2 µm/m-°C @Temperature 20.0 - 300 °C | 6.78 µin/in-°F @Temperature 68.0 - 572 °F |
| 13.3 µm/m-°C @Temperature 20.0 - 400 °C | 7.39 µin/in-°F @Temperature 68.0 - 752 °F |
| 13.9 µm/m-°C @Temperature 20.0 - 500 °C | 7.72 µin/in-°F @Temperature 68.0 - 932 °F |
| 14.2 µm/m-°C @Temperature 20.0 - 600 °C | 7.89 µin/in-°F @Temperature 68.0 - 1110 °F |
| 14.8 µm/m-°C @Temperature 20.0 - 700 °C | 8.22 µin/in-°F @Temperature 68.0 - 1290 °F |
Specific Heat Capacity | 0.486 J/g-°C @Temperature >=100 °C | 0.116 BTU/lb-°F @Temperature >=212 °F |
| 0.515 J/g-°C @Temperature 150 - 200 °C | 0.123 BTU/lb-°F @Temperature 302 - 392 °F |
| 0.528 J/g-°C @Temperature 200 - 250 °C | 0.126 BTU/lb-°F @Temperature 392 - 482 °F |
| 0.548 J/g-°C @Temperature 250 - 300 °C | 0.131 BTU/lb-°F @Temperature 482 - 572 °F |
| 0.569 J/g-°C @Temperature 300 - 350 °C | 0.136 BTU/lb-°F @Temperature 572 - 662 °F |
| 0.586 J/g-°C @Temperature 350 - 400 °C | 0.140 BTU/lb-°F @Temperature 662 - 752 °F |
| 0.624 J/g-°C @Temperature 750 - 800 °C | 0.149 BTU/lb-°F @Temperature 1380 - 1470 °F |
| 0.649 J/g-°C @Temperature 450 - 500 °C | 0.155 BTU/lb-°F @Temperature 842 - 932 °F |
| 0.708 J/g-°C @Temperature 550 - 600 °C | 0.169 BTU/lb-°F @Temperature 1020 - 1110 °F |
| 0.770 J/g-°C @Temperature 650 - 700 °C | 0.184 BTU/lb-°F @Temperature 1200 - 1290 °F |
| 1.583 J/g-°C @Temperature 700 - 750 °C | 0.3783 BTU/lb-°F @Temperature 1290 - 1380 °F |
Thermal Conductivity | 24.7 W/m-K @Temperature 800 °C | 171 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 29.8 W/m-K @Temperature 1200 °C | 207 BTU-in/hr-ft²-°F @Temperature 2190 °F |
| 30.1 W/m-K @Temperature 700 °C | 209 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 32.9 W/m-K @Temperature 1000 °C | 228 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 33.9 W/m-K @Temperature 600 °C | 235 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 38.2 W/m-K @Temperature 500 °C | 265 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 41.7 W/m-K @Temperature 400 °C | 289 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 45.7 W/m-K @Temperature 300 °C | 317 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 48.1 W/m-K @Temperature 200 °C | 334 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 50.7 W/m-K @Temperature 100 °C | 352 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 51.9 W/m-K @Temperature 0.000 °C | 360 BTU-in/hr-ft²-°F @Temperature 32.0 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.37 - 0.44 % | 0.37 - 0.44 % |
Iron, Fe | 98.6 - 99 % | 98.6 - 99 % |
Manganese, Mn | 0.60 - 0.90 % | 0.60 - 0.90 % |
Phosphorus, P | <= 0.040 % | <= 0.040 % |
Sulfur, S | <= 0.050 % | <= 0.050 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.