MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sandvik Bioline Ti6Al4V ELI Bar
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Beta Titanium Alloy

Material Notes: Sandvik Bioline Ti6Al4V ELI is an alphabeta titanium alloy mainly used for medical implant applications. It is an Extra Low Interstitial alloy with a high purity, which confers improved ductility and fracture toughness. The grade meets the stringent requirements of all applicable standards for implant materials. Sandvik Bioline Ti6Al4V ELI is characterized by:
  • Excellent biocompatibility
  • Good forgeability
  • Advanced corrosion resistance
  • High strength
  • High purity
  • A high quality surface finish

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 3131
Tensile Strength, Ultimate 940 MPa136000 psi
 >= 825 MPa
@Thickness 44.45 - 63.5 mm
>= 120000 psi
@Thickness 1.750 - 2.50 in
ASTM F136
 >= 860 MPa
@Thickness <=44.45 mm
>= 125000 psi
@Thickness <=1.750 in
ASTM F136
Tensile Strength, Yield 870 MPa
@Strain 0.2 %
126000 psi
@Strain 0.2 %
 >= 760 MPa
@Strain 0.2 %,
Thickness 44.45 - 63.5 mm
>= 110000 psi
@Strain 0.2 %,
Thickness 1.750 - 2.50 in
ASTM F136
 >= 795 MPa
@Strain 0.2 %,
Thickness <=44.45 mm
>= 115000 psi
@Strain 0.2 %,
Thickness <=1.750 in
ASTM F136
Elongation at Break 15 %15 %in 5D
 16 %16 %in 4D
 >= 8.0 %
@Thickness 44.45 - 63.5 mm
>= 8.0 %
@Thickness 1.750 - 2.50 in
in 4D, ASTM F136
 >= 10 %
@Thickness <=44.45 mm
>= 10 %
@Thickness <=1.750 in
in 4D, ASTM F136
Reduction of Area 39 %39 %
 >= 20 %
@Thickness 44.45 - 63.5 mm
>= 20 %
@Thickness 1.750 - 2.50 in
20
 >= 25 %
@Thickness <=44.45 mm
>= 25 %
@Thickness <=1.750 in
25
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 5.5 - 6.5 %5.5 - 6.5 %
Carbon, C <= 0.080 %<= 0.080 %
Hydrogen, H <= 0.012 %<= 0.012 %
Iron, Fe <= 0.25 %<= 0.25 %
Nitrogen, N <= 0.050 %<= 0.050 %
Oxygen, O <= 0.13 %<= 0.13 %
Titanium, Ti 88.48 - 91 %88.48 - 91 %
Vanadium, V 3.5 - 4.5 %3.5 - 4.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-6Al-4V ELI (Grade 23), Annealed
Titanium Ti-6Al-4V (Grade 5), Annealed
Titanium Ti-6Al-4V (Grade 5), STA
Titanium Ti-6Al-4V (Grade 5), STA Bar
Arcam Ti6Al4V Titanium Alloy

NSANDV5206 / 199770

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.