MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Latrobe Lescalloy® BG42 VIM-VAR High Performance Bearing Steel
Categories: Metal; Ferrous Metal; Martensitic; Stainless Steel

Material Notes: LESCALLOY BG42 VIM-VAR steel is a martensitic, stainless high speed steel that combines the tempering, hot hardness and hardness retention characteristics of M50 high speed steel with the corrosion and oxidation resistance of type 440C stainless. LESCALLOY BG42 VIM-VAR is double vacuum melted (vacuum induction followed by VAC-ARC® remelting) to consistently assure good cleanliness and superior properties. Although often used for aerospace bearings and other critical applications, its excellent wear resistance and corrosion resistance makes it a superior choice for use in cutlery applications.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.75 g/cc0.280 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C  56.5
@Temperature 482 °C
56.5
@Temperature 900 °F
 60
@Temperature 316 °C
60
@Temperature 600 °F
 63
@Temperature 93.3 °C
63
@Temperature 200 °F
Modulus of Elasticity 220.6 GPa31990 ksi
 180.6 GPa
@Temperature 482 °C
26190 ksi
@Temperature 900 °F
Modulus of Rigidity 70.40 GPa10210 ksiAt 900°F
 86.53 GPa12550 ksiAt 78°F
Poissons Ratio 0.270.27
Machinability 55 - 60 %55 - 60 %1% Carbon Steel
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.81 µm/m-°C
@Temperature -73.0 - 21.0 °C
5.45 µin/in-°F
@Temperature -99.4 - 69.8 °F
 11.03 µm/m-°C
@Temperature 21.0 - 149 °C
6.128 µin/in-°F
@Temperature 69.8 - 300 °F
 12.33 µm/m-°C
@Temperature 21.0 - 538 °C
6.850 µin/in-°F
@Temperature 69.8 - 1000 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 1.15 %1.15 %
Chromium, Cr 14.5 %14.5 %
Iron, Fe 78.35 %78.35 %
Manganese, Mn 0.50 %0.50 %
Molybdenum, Mo 4.0 %4.0 %
Silicon, Si 0.30 %0.30 %
Vanadium, V 1.2 %1.2 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Latrobe Lescalloy® M50 VIM-VAR High Performance Bearing Steel
Latrobe Lescalloy® 52100 VAC-ARC High Performance Bearing Steel
BG42 High Performance Bearing Steel
Latrobe BG42® Stainless Knife Steel (AMS 5749)
Latrobe CSS-42L™ VIM-VAR High Performance Carburizing Stainless Steel; Bearing and Gear Steel

NTIMK002 / 19350

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.