MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

INEOS Styrolution Lustran® 256/Lustran® 752 Blended ABS Resin
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Impact Grade, Molded

Material Notes: 50/50 pellet blend of Lustran® 256 ABS and high-impact Lustran® 752 ABS

Information provided by the manufacturer.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 34.0 MPa4930 psiASTM-D638
Tensile Modulus 2.00 GPa290 ksiASTM-D638
Flexural Yield Strength 61.0 MPa8850 psiASTM-D790
Flexural Modulus 2.00 GPa290 ksiASTM-D790
Izod Impact, Notched  0.910 J/cm
@Thickness 3.20 mm,
Temperature -40.0 °C
1.70 ft-lb/in
@Thickness 0.126 in,
Temperature -40.0 °F
ASTM-D256
 1.60 J/cm
@Thickness 3.20 mm,
Temperature -18.0 °C
3.00 ft-lb/in
@Thickness 0.126 in,
Temperature -0.400 °F
ASTM-D256
 2.99 J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
5.60 ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM-D256
Instrumented Impact Total Energy  19.0 J
@Temperature -40.0 °C
14.0 ft-lb
@Temperature -40.0 °F
Instrumented Impact (0.5-in. dart, 3-in. clamp, 7.6 mph); ASTM-D3763
 26.0 J
@Temperature -18.0 °C
19.2 ft-lb
@Temperature -0.400 °F
Instrumented Impact (0.5-in. dart, 3-in. clamp, 7.6 mph); ASTM-D3763
 43.0 J
@Temperature 23.0 °C
31.7 ft-lb
@Temperature 73.4 °F
Instrumented Impact (0.5-in. dart, 3-in. clamp, 7.6 mph); ASTM-D3763
Instrumented Impact Energy at Peak  18.0 J
@Temperature -40.0 °C
13.3 ft-lb
@Temperature -40.0 °F
Instrumented Impact (0.5-in. dart, 3-in. clamp, 7.6 mph); ASTM-D3763
 23.0 J
@Temperature -18.0 °C
17.0 ft-lb
@Temperature -0.400 °F
Instrumented Impact (0.5-in. dart, 3-in. clamp, 7.6 mph); ASTM-D3763
 31.0 J
@Temperature 23.0 °C
22.9 ft-lb
@Temperature 73.4 °F
Instrumented Impact (0.5-in. dart, 3-in. clamp, 7.6 mph); ASTM-D3763
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C185 °FUnannealed; ASTM-D648
 
Optical PropertiesMetricEnglishComments
Gloss 40 %40 %Formed, Angle 60°; ASTM-D523
 85 %85 %Sheet, Angle 60°; ASTM-D523

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman Diamond Centrex® 814 General Purpose Injection Molding Grade
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Impact Grade, Molded
Lotte Advanced Materials Starex® SR-7300 ABS/PET, Unreinforced
Polyram RamLloy PJ701 ABS/ASA, General Purpose
Polyram RamShine PV701 ABS, UV Stabilized

PINEA956 / 107227

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.