MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow TUFLIN™ HS-7065 NT 7 Linear Low Density Polyethylene Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE)

Material Notes:
  • Hexene Linear Low Density Resin
  • Good Processability at Narrow Die Gaps
  • Complies with U.S. FDA 21 CFR 177.1520 (c) 3.2a
TUFLIN™ HS-7065 NT 7 is a fractional melt, ethylene-hexene copolymer, designed for good toughness and stiffness. This product is recommended for thin and thick gauge applications such as trash bags and heavy-duty shipping sacks that require strength and output.

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.9289 g/cc0.03356 lb/in³ASTM D792
Thickness 20.3 microns0.800 mil
Melt Flow 0.80 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.80 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
Antiblock Level 4000 ppm4000 ppm
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 16.62 MPa2411 psiASTM D882
Film Tensile Strength at Yield, TD 19.59 MPa2841 psiASTM D882
Film Elongation at Break, MD 703 %703 %ASTM D882
Film Elongation at Break, TD 793 %793 %ASTM D882
Secant Modulus, MD 0.2986 GPa43.31 ksi2% Secant; ASTM D882
Secant Modulus, TD 0.2830 GPa41.04 ksi2% Secant; ASTM D882
Impact 1010[lbf]; Puncture Resistance Force; Dow Method
 101101[ft-lbf/in3]; Puncture Resistance; Dow Method
 37013701[ft-lbf/in3]; Toughness MD; ASTM D882
 48324832[ft-lbf/in3]; Toughness TD; ASTM D882
Puncture Energy 2.15 J1.58 ft-lbDow Method
Elmendorf Tear Strength MD 171 g171 gMethod B; ASTM D1922
Elmendorf Tear Strength TD 715 g715 gMethod B; ASTM D1922
Elmendorf Tear Strength, MD 8.4153 g/micron213.75 g/milASTM D1922
Elmendorf Tear Strength, TD 35.187 g/micron893.75 g/milASTM D1922
Dart Drop Test 55.0 g0.121 lbMethod A; ASTM D1709
 <= 100 g<= 0.221 lbMethod B; ASTM D1709
Film Tensile Strength at Break, MD 48.53 MPa7038 psiASTM D882
Film Tensile Strength at Break, TD 54.01 MPa7833 psiASTM D882
Heat Seal Strength, Ultimate 13.3 N2.99 lb (f)at 140°C, 0.5 sec dwell, 40 psi bar pressure, pull speed 10 (in./min.); Dow Method
Heat Seal Strength Initiation Temperature 120 °C248 °F1 lb/in heat seal strength; 0.5 sec dwell, 40 psi bar pressure, pull speed 10 (in./min.); Dow Method
 
Thermal PropertiesMetricEnglishComments
Melting Point 126 °C259 °FDow Method (DSC)
Vicat Softening Point 116 °C241 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 9.0 %9.0 %ASTM D1003
Gloss 73 %73 %45°; ASTM D2457
 77 %77 %20°; ASTM D2457
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow TUFLIN™ HS-7041 NT 7 Linear Low Density Polyethylene Resin
Dow TUFLIN™ HS-7066 NT 7 Linear Low Density Polyethylene Resin
Dow TUFLIN™ HS-7094 NT 7 Linear Low Density Polyethylene Resin
Dow LDPE 641I Low Density Polyethylene, Liner Film Grade
Dow TUFLIN™ HS-7021 NT 7 Linear Low Density Polyethylene Resin

PDOW1446 / 30664

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.