MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Industeel SOLEIL A2 13% Cr High Strength Martensitic Stainless Steel (QT650 Heat Treatment)
Categories: Metal; Ferrous Metal; Martensitic; Stainless Steel; T S40000 Series Stainless Steel

Material Notes: Description: Soleil A2 has combined Chromium (~13%) and Carbon ~0.10%) additions to provide an excellent combination of high mechanical properties and improved corrosion resistance properties. The grade has a martensitic microstructure. The final mechanical properties may be optimized by selecting an appropriate heat treatment. In the annealed conditions the alloy presents ductility and may be formed. Chromium additions (~13%) improve the corrosion resistance, particularly in wet conditions when compared to C-Mn steels. Slightly acidified and abrasion conditions are considered. The main applications concern mechanical industry, oil and gas industry, sugar industry and constructional components.

Information provided by manufacturer.

Key Words: EURONORM 1.4006 X12 Cr 13, AFNOR Z 12 C 13, DIN W 1.4006 (DIN 17440), ASTM A240 TP 410, UNS S41000
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.70 g/cc0.278 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 190190Typical
Tensile Strength, Ultimate 650 - 850 MPa94300 - 123000 psiMinimum Guaranteed
Tensile Strength, Yield >= 450 MPa>= 65300 psiMinimum Guaranteed
Elongation at Break >= 12 %>= 12 %
Modulus of Elasticity 212 GPa30700 ksi
Charpy Impact 70.0 J51.6 ft-lbTypical Toughness (long)
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000600 ohm-cm
@Temperature 20.0 °C
0.0000600 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.5 µm/m-°C
@Temperature 20.0 - 100 °C
5.83 µin/in-°F
@Temperature 68.0 - 212 °F
 11.0 µm/m-°C
@Temperature 20.0 - 200 °C
6.11 µin/in-°F
@Temperature 68.0 - 392 °F
 11.5 µm/m-°C
@Temperature 20.0 - 300 °C
6.39 µin/in-°F
@Temperature 68.0 - 572 °F
 12.0 µm/m-°C
@Temperature 20.0 - 500 °C
6.67 µin/in-°F
@Temperature 68.0 - 932 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 20.0 °C
0.110 BTU/lb-°F
@Temperature 68.0 °F
Thermal Conductivity 25.0 W/m-K
@Temperature 20.0 °C
174 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.12 %0.12 %
Chromium, Cr 12.5 %12.5 %
Iron, Fe 86.48 %86.48 %As remainder
Manganese, Mn 0.50 %0.50 %
Silicon, Si 0.40 %0.40 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Industeel SOLEIL A2 13% Cr High Strength Martensitic Stainless Steel (QT550 Heat Treatment)
410 Stainless Steel
410 Cb Martensitic Stainless Steel (UNS S41040)
410 Stainless Steel, tempered at 623°C
AK Steel ZINCGRIP® 275, Grade 40 Hot Dip Galvanized Carbon Steel, Structural Steel (SS)

NINDUST18 / 17556

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.