MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

INEOS Styrolution Empera® 524G Polystyrene  (discontinued **)
Categories: Polymer; Thermoplastic; Polystyrene (PS)

Material Notes: Empera® 524N is a ground version of Empera® 524N, an impact polystyrene with good flow properties.
    Features:
  • Good Flow
  • High Impact Resistance
Uses:
  • Compounding
  • MasterbatchAgency Ratings: EU 10/2011

    RoHS Compliance: Contact Manufacturer

      Processing Method:
    • Compounding

  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 1.04 g/cc0.0376 lb/in³ISO 1183
    Water Absorption <= 0.10 %
    @Temperature 23.0 °C,
    Time 86400 sec
    <= 0.10 %
    @Temperature 73.4 °F,
    Time 24.0 hour
    ISO 62
    Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inISO 294-4
    Melt Flow 10.5 g/10 min
    @Load 5.00 kg,
    Temperature 200 °C
    10.5 g/10 min
    @Load 11.0 lb,
    Temperature 392 °F
    ISO 1133
     
    Mechanical PropertiesMetricEnglishComments
    Ball Indentation Hardness 100 MPa14500 psiH 358/30; ISO 2039-1
    Tensile Strength at Break 23.0 MPa3340 psiISO 527-2/50
    Tensile Strength, Yield 26.0 MPa3770 psiISO 527-2/50
    Elongation at Break 50 %50 %ISO 527-2/50
    Elongation at Yield 1.2 %1.2 %ISO 527-2/50
    Tensile Modulus 2.10 GPa305 ksiISO 527-2/1
    Flexural Strength 40.0 MPa5800 psi2.0 mm/min; ISO 178
    Charpy Impact Unnotched 0.800 J/cm²3.81 ft-lb/in²ISO 179/1eU
     
    Thermal PropertiesMetricEnglishComments
    CTE, linear, Parallel to Flow 80.0 µm/m-°C
    @Temperature 23.0 - 80.0 °C
    44.4 µin/in-°F
    @Temperature 73.4 - 176 °F
    DIN 53752
    Thermal Conductivity 0.160 W/m-K1.11 BTU-in/hr-ft²-°FDIN 52612
    Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C176 °FUnannealed; ISO 75-2/A
    Vicat Softening Point 85.0 °C185 °FISO 306/B50

    **
    Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

    Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    INEOS Styrolution Polystyrol 143 E GR 2 PS
    INEOS Styrolution Polystyrol 143 E GR 21 PS
    INEOS Styrolution Empera® 433N Polystyrene
    INEOS Styrolution 156F Polystyrene
    INEOS Styrolution Terlux® 2802 Transparent MABS

    PZZSTYR991 / 209792

    Aluminum Castings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.