MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

RTP Company RTP 152 HF Polypropylene (PP), High Flow - Flame Retardant - UL94 V-2
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Flame Retardant

Material Notes: The RTP 152 family of compounds are flame retarded, unreinforced polypropylene materials. They offer excellent moldability, non-corrosive characteristics and the living-hinge effect.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.930 g/cc0.930 g/ccASTM D 792
Water Absorption 0.010 %0.010 %24 hrs @ 23°C; ASTM D 570
Linear Mold Shrinkage 0.015 - 0.020 cm/cm
@Thickness 3.17 mm
0.015 - 0.020 in/in
@Thickness 0.125 in
ASTM D955
Melt Flow 18 - 24 g/10 min
@Load 2.16 kg,
Temperature 230 °C
18 - 24 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D 1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 30.3 MPa4400 psiASTM D 638
Elongation at Break >= 100 %>= 100 %ASTM D 638
Tensile Modulus 1.59 GPa230 ksiASTM D 638
Flexural Strength 35.9 MPa5200 psiASTM D 790
Flexural Modulus 1.24 GPa180 ksiASTM D 790
Izod Impact, Notched 0.267 J/cm
@Thickness 3.17 mm
0.500 ft-lb/in
@Thickness 0.125 in
D 256
Izod Impact, Unnotched 9.61 J/cm
@Thickness 3.17 mm
18.0 ft-lb/in
@Thickness 0.125 in
ASTM D4812
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmASTM D 257
Dielectric Strength 19.7 kV/mm500 kV/inShort Term; in oil; ASTM D 149
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 51.7 °C125 °FASTM D 648
Flammability, UL94 V-2
@Thickness 0.7937 mm
V-2
@Thickness 0.03125 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 191 - 232 °C375 - 450 °F
Mold Temperature 32.2 - 65.6 °C90.0 - 150 °F
Drying Temperature 79.4 °C175 °F
Dry Time 2 hour2 hour
Injection Pressure 68.9 - 103 MPa10000 - 15000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RTP Company RTP 150 HF Polypropylene (PP), High Flow - Unreinforced - Flame Retardant - UL94 V-0
RTP Company RTP 199 X 137777 C Polypropylene (PP) Copolymer - High Flow - High Impact - Flame Retardant - UV Stabilized
BYK PRIEX® 25093 Maleic Anhydride Grafted PP random copolymer
North Wood Plastics HDPE with 20% Wood Fiber
RTP Company RTP 199 X 132495 B Polypropylene (PP), High Flow - Cellulose Fiber - 30% Renewable Resource Content

PQZWA837 / 92371

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.