BASF Procom® GC30S 401 Polypropylene
Categories:
Polymer
;
Thermoplastic
;
Polypropylene (PP)
;
Polypropylene, Molded
Material Notes:
Uses: Electrical appliance housings (e.g. drills), components requiring high impact and temperature resistance, furniture frames.
Data was collected by ISO methods and provided by BASF.
Key Words:
PP
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.12
g/cc
0.0405
lb/in³
Linear Mold Shrinkage, Flow
0.0060
cm/cm
0.0060
in/in
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
61.0
MPa
8850
psi
Elongation at Break
3.5 %
3.5 %
Tensile Modulus
5.70
GPa
827
ksi
Charpy Impact Unnotched
5.50
J/cm²
26.2
ft-lb/in²
5.00
J/cm²
@Temperature -30.0 °C
23.8
ft-lb/in²
@Temperature -22.0 °F
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
30.0
µm/m-°C
@Temperature 20.0 °C
16.7
µin/in-°F
@Temperature 68.0 °F
Deflection Temperature at 0.46 MPa (66 psi)
159
°C
318
°F
Deflection Temperature at 1.8 MPa (264 psi)
140
°C
284
°F
Vicat Softening Point
100
°C
212
°F
Flammability, UL94
HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
BASF Procom® D 1118 Polypropylene
BASF Procom® D 1153 Polypropylene
BASF Procom® D 1146 Polypropylene
BASF Procom® D 1133 Polypropylene
BASF Procom® D 1085 Polypropylene
PSF219 / 66800
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.