MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ineos K44-15-122 HDPE
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE)

Material Notes: K44-15-122 is a natural high density polyethylene copolymer designed specifically for extrusion of pipe. It has NSF Standard 14 certification for potable water applications, complies with ANSI/NSF Standard 61 health effects requirements, and is recognized by the Plastic Pipe Institute as having a pipe material designation code of PE 3608 (formerly PE 3408). A pressure rated formulation is also produced when this product is extruded in combination with a Ineos approved black masterbatch. The resulting formulation known as K44-15-123 has NSF Standard 14 certification and complies with ANSI/NSF Standard 61 health effects requirements, is certified to CSA Standard B137.1-05 and B137.4-05, and is listed with the Plastic Pipe Institute as a PE 3608(formerly PE 3408) and PE 80 pipe material designation code.

Key Words: Natural PE 3608 pipe grade, meets ANSI/NSF Standard
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.944 g/cc0.0341 lb/in³Natural; ASTM D4883
Environmental Stress Crack Resistance >= 2000 hour>= 2000 hourCondition B; ASTM D1693
 >= 5000 hour>= 5000 hourCondition C; ASTM D1693
High Load Melt Index 12.5 g/10 min12.5 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
PENT >= 100 hour>= 100 hourNotch Tensile; ASTM F1473
Hardness, Shore D 6868ASTM D2240
Tensile Strength at Break 31.0 MPa4500 psi2 in/min.; ASTM D638
Tensile Strength, Yield 22.8 MPa3310 psi2 in/min.; ASTM D638
Elongation at Break >= 800 %>= 800 %2 in/min.; ASTM D638
Flexural Modulus 0.827 GPa
@Strain 2 %
120 ksi
@Strain 2 %
Secant-Method 1; ASTM D790
Izod Impact, Notched 3.20 J/cm5.99 ft-lb/inASTM D256
Hydrostatic Design Basis 11.0 MPa1600 psiASTM D2837
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 126 °C259 °FASTM D1525
Brittleness Temperature <= -118 °C<= -180 °FASTM D746
 
Descriptive Properties
processColor Concentrate

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ineos TUB 121N HDPE
Ineos K44-08-122 HDPE
Ineos K44-15-186 Polyethylene Copolymer
Ineos TUB 121NTW HDPE
Special Metals NILO® Alloy 36 Low-Expansion Alloy

PSOLKM014 / 68245

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.