MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

CENTROPLAST CENTROLEN PE-UHMW Ultra-high molecular weight polyethylene
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); UHMW PE (Ultra High Molecular Weight PE)

Material Notes: This plastic is a low density, easily machined material that can be welded and has a low sliding friction with high impact resistance. Applications include glide strips, pump components, and wearing parts.

Information provided by CENTROPLAST Engineering Plastics GMBH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.940 g/cc0.0340 lb/in³ISO 1183
Water Absorption at Saturation 0.010 %0.010 %in water at 23°C; ISO 62
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 40.0 MPa5800 psivalue at 30 sec.; ISO 2039-1
Tensile Strength, Yield 20.0 MPa2900 psiv = 50 mm/min; ISO 527-2
Elongation at Break >= 50 %>= 50 %ISO 527-2
Tensile Modulus 0.800 GPa116 ksiISO 527-2
Charpy Impact Unnotched NBNBISO 179/1eU
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 60093
Dielectric Constant  2.3
@Frequency 100 Hz
2.3
@Frequency 100 Hz
IEC 60250
 3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 45.0 kV/mm1140 kV/inin transformer oil; IEC 60243-1
Dissipation Factor  0.00040
@Frequency 100 Hz
0.00040
@Frequency 100 Hz
IEC 60250
 0.0010
@Frequency 1e+6 Hz
0.0010
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 200 µm/m-°C
@Temperature 20.0 °C
111 µin/in-°F
@Temperature 68.0 °F
ISO 11359
Thermal Conductivity 0.410 W/m-K2.85 BTU-in/hr-ft²-°F
Melting Point 135 °C275 °F10K/min; ISO 3146
Maximum Service Temperature, Air 80.0 °C176 °FLong Term
 120 °C248 °FShort term
Deflection Temperature at 1.8 MPa (264 psi) 42.0 °C108 °FISO 75-2
Vicat Softening Point 80.0 °C176 °FVST/B/50; ISO 306
Minimum Service Temperature, Air -200 °C-328 °F
Flammability, UL94  HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 HB
@Thickness 6.00 mm
HB
@Thickness 0.236 in
 
Compliance PropertiesMetricEnglishComments
FDA YesYesFood Compliance
 
Descriptive Properties
Food ComplianceyesBGVV

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Braskem UTEC® 3040 Ultra High Molecular Weight Polyethylene
Braskem UTEC® 4040 Ultra High Molecular Weight Polyethylene
Garland Manufacturing GAR-DUR® Ultra High Molecular Weight Polyethylene (UHMW-PE)
Mitsubishi Chemical Advanced Materials TIVAR™ 1000 Virgin UHMW-PE, (Natural & Colors except Black)
Röchling LAMIGAMID® 700 Ultra High Molecular Weight Polyethylene

PCENTR29 / 27980

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.