MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Texin® 285 Thermoplastic Polyurethanes (TPU)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Texin 285 resin is an aromatic polyester-based thermoplastic polyurethane with a Shore hardness of approximately 85A. It can be processed by injection molding, extrusion, and blow molding.

Properties / Applications: In addition to good clarity, Texin 285 resin offers outstanding abrasion resistance, impact strength, toughness, and exibility. Texin 285 natural color resin complies with FDA food-contact regulations 21 CFR 177.1680 (Polyurethane Resins) and 177.2600 (Rubber Articles Intended for Repeated Use), subject to the limitations of these and any other applicable regulations. Typical applications include belting, tubing, hose, cable jackets, hose jackets, seals, athletic soles, casters, mine screens, film, and extruded profiles. Texin 285 resin can also be used as a polymer modifier.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8585ASTM D2240
Tensile Strength at Break 37.9 MPa5500 psiASTM D412
Tensile Stress at Strain  5.00 MPa
@Strain 50 %
725 psi
@Strain 50 %
ASTM D412
 5.30 MPa
@Strain 100 %
769 psi
@Strain 100 %
ASTM D412
 13.1 MPa
@Strain 300 %
1900 psi
@Strain 300 %
ASTM D412
Elongation at Break 500 %500 %ASTM D412
Flexural Modulus  0.0276 GPa
@Temperature 23.0 °C
4.00 ksi
@Temperature 73.4 °F
ASTM D790
 0.0496 GPa
@Temperature -30.0 °C
7.19 ksi
@Temperature -22.0 °F
ASTM D790
Compressive Strength 0.300 MPa43.5 psi2% Deflection; ASTM D 575
 1.00 MPa145 psi5% Deflection; ASTM D 575
 2.20 MPa319 psi10% Deflection; ASTM D 575
 3.30 MPa479 psi15% Deflection; ASTM D 575
 4.30 MPa624 psi20% Deflection; ASTM D 575
 5.70 MPa827 psi25% Deflection; ASTM D 575
 15.0 MPa2180 psi50% Deflection; ASTM D 575
Resilience 4545[%], Bayshore; ASTM D2632
Tear Strength 87.6 kN/m500 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 35
@Load 1.00 kg
35
@Load 2.20 lb
[mg] Loss, H-18; ASTM D3489
Compression Set  12 %
@Temperature 23.0 °C,
Time 79200 sec
12 %
@Temperature 73.4 °F,
Time 22.0 hour
postcured; ASTM D395-B
 16 %
@Temperature 23.0 °C,
Time 79200 sec
16 %
@Temperature 73.4 °F,
Time 22.0 hour
as molded; ASTM D395-B
 35 %
@Temperature 70.0 °C,
Time 79200 sec
35 %
@Temperature 158 °F,
Time 22.0 hour
postcured; ASTM D395-B
 65 %
@Temperature 70.0 °C,
Time 79200 sec
65 %
@Temperature 158 °F,
Time 22.0 hour
as molded; ASTM D395-B
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 91.0 °C196 °FRate A; ASTM D1525
Brittleness Temperature >= -55.6 °C>= -68.0 °FASTM D746
Glass Transition Temp, Tg -42.0 °C-43.6 °F
UL RTI, Electrical 50.0 °C122 °FUL 746B
UL RTI, Mechanical with Impact 50.0 °C122 °FUL 746B
UL RTI, Mechanical without Impact 50.0 °C122 °FUL 746B
Flammability, UL94  HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 V-2
@Thickness 3.00 mm
V-2
@Thickness 0.118 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 180 - 200 °C356 - 392 °FInjection
 180 - 200 °C356 - 392 °FExtrusion
Middle Barrel Temperature 180 - 205 °C356 - 401 °FInjection
 180 - 205 °C356 - 401 °FExtrusion
Front Barrel Temperature 180 - 210 °C356 - 410 °FInjection
 180 - 210 °C356 - 410 °FExtrusion
Nozzle Temperature 185 - 210 °C365 - 410 °FInjection
Adapter Temperature 180 - 210 °C356 - 410 °FExtrusion
Die Temperature 185 - 210 °C365 - 410 °FExtrusion
Melt Temperature 190 - 205 °C374 - 401 °FExtrusion
 195 - 205 °C383 - 401 °FInjection
Mold Temperature 15.0 - 40.0 °C59.0 - 104 °F
Injection Pressure 41.4 - 103 MPa6000 - 15000 psiInjection
Back Pressure <= 1.38 MPa<= 200 psiInjection
Cushion <= 0.317 cm<= 0.125 inInjection
 
Compliance PropertiesMetricEnglishComments
FDA YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lubrizol ESTANE® 54610 Ester Based Thermoplastic Polyurethane
Covestro Texin® 270 Thermoplastic Polyurethanes (TPU)
BASF Ultramid® 1310-11 NF2001 PA66 (Dry)
Covestro Desmopan® DP 9370A Polyurethane
BASF Elastollan® C 85 A HPM TPUR

PCOVEST0979 / 202762

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.