MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes HR-120® alloy, solution heat-treated plate
Categories: Metal; Superalloy; Iron Base

Material Notes: Excellent strength at elevated temperatures, combined with good resistance to carburizing and sulfidizing environments. Applications include bar frame heat treating baskets, wire mesh furnace belts and basket liners, muffles and retorts, heat treating fixtures, waste incinerators, radiant tubes, cast link belt pins, recuperators, and fluidized bed components.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: ASTM B514, ASTM B407, ASTM B515, ASTM B564, ASTM B366, DIN No.2.4854, UNS N08120, ASTM B163, ASTM B408, ASTM B409
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.07 g/cc0.292 lb/in³at RT.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 735 MPa107000 psi
 34.0 MPa
@Temperature 1205 °C
4930 psi
@Temperature 2201 °F
 105 MPa
@Temperature 1095 °C
15200 psi
@Temperature 2003 °F
 190 MPa
@Temperature 980 °C
27600 psi
@Temperature 1800 °F
 325 MPa
@Temperature 870 °C
47100 psi
@Temperature 1600 °F
 440 MPa
@Temperature 760 °C
63800 psi
@Temperature 1400 °F
 505 MPa
@Temperature 650 °C
73200 psi
@Temperature 1200 °F
 555 MPa
@Temperature 540 °C
80500 psi
@Temperature 1000 °F
Tensile Strength, Yield 375 MPa
@Strain 0.2 %
54400 psi
@Strain 0.2 %
 27.0 MPa
@Strain 0.2 %,
Temperature 1205 °C
3920 psi
@Strain 0.2 %,
Temperature 2201 °F
 63.0 MPa
@Strain 0.2 %,
Temperature 1095 °C
9140 psi
@Strain 0.2 %,
Temperature 2003 °F
 135 MPa
@Strain 0.2 %,
Temperature 980 °C
19600 psi
@Strain 0.2 %,
Temperature 1800 °F
 170 MPa
@Strain 0.2 %,
Temperature 650 °C
24700 psi
@Strain 0.2 %,
Temperature 1200 °F
 175 MPa
@Strain 0.2 %,
Temperature 760 °C
25400 psi
@Strain 0.2 %,
Temperature 1400 °F
 175 MPa
@Strain 0.2 %,
Temperature 540 °C
25400 psi
@Strain 0.2 %,
Temperature 1000 °F
 185 MPa
@Strain 0.2 %,
Temperature 870 °C
26800 psi
@Strain 0.2 %,
Temperature 1600 °F
Elongation at Break 50 %50 %in 50.8 mm
 50 %
@Temperature 760 °C
50 %
@Temperature 1400 °F
in 50.8 mm
 51 %
@Temperature 870 °C
51 %
@Temperature 1600 °F
in 50.8 mm
 60 %
@Temperature 650 °C
60 %
@Temperature 1200 °F
in 50.8 mm
 61 %
@Temperature 540 °C
61 %
@Temperature 1000 °F
in 50.8 mm
 81 %
@Temperature 980 °C
81 %
@Temperature 1800 °F
in 50.8 mm
 89 %
@Temperature 1095 °C
89 %
@Temperature 2003 °F
in 50.8 mm
 89 %
@Temperature 1205 °C
89 %
@Temperature 2201 °F
in 50.8 mm
Modulus of Elasticity 197 GPa28600 ksiRT
 128 GPa
@Temperature 1000 °C
18600 ksi
@Temperature 1830 °F
 136 GPa
@Temperature 900 °C
19700 ksi
@Temperature 1650 °F
 143 GPa
@Temperature 800 °C
20700 ksi
@Temperature 1470 °F
 152 GPa
@Temperature 700 °C
22000 ksi
@Temperature 1290 °F
 159 GPa
@Temperature 600 °C
23100 ksi
@Temperature 1110 °F
 165 GPa
@Temperature 500 °C
23900 ksi
@Temperature 932 °F
 174 GPa
@Temperature 400 °C
25200 ksi
@Temperature 752 °F
 182 GPa
@Temperature 300 °C
26400 ksi
@Temperature 572 °F
 188 GPa
@Temperature 200 °C
27300 ksi
@Temperature 392 °F
 194 GPa
@Temperature 100 °C
28100 ksi
@Temperature 212 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0001052 ohm-cm0.0001052 ohm-cmRT
 0.0001231 ohm-cm
@Temperature 700 °C
0.0001231 ohm-cm
@Temperature 1290 °F
 0.0001245 ohm-cm
@Temperature 800 °C
0.0001245 ohm-cm
@Temperature 1470 °F
 0.0001257 ohm-cm
@Temperature 900 °C
0.0001257 ohm-cm
@Temperature 1650 °F
 0.0001266 ohm-cm
@Temperature 1000 °C
0.0001266 ohm-cm
@Temperature 1830 °F
 0.0001278 ohm-cm
@Temperature 1100 °C
0.0001278 ohm-cm
@Temperature 2010 °F
 0.0001287 ohm-cm
@Temperature 1200 °C
0.0001287 ohm-cm
@Temperature 2190 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.3 µm/m-°C
@Temperature 25.0 - 100 °C
7.94 µin/in-°F
@Temperature 77.0 - 212 °F
 14.9 µm/m-°C
@Temperature 25.0 - 200 °C
8.28 µin/in-°F
@Temperature 77.0 - 392 °F
 15.3 µm/m-°C
@Temperature 25.0 - 300 °C
8.50 µin/in-°F
@Temperature 77.0 - 572 °F
 15.8 µm/m-°C
@Temperature 25.0 - 400 °C
8.78 µin/in-°F
@Temperature 77.0 - 752 °F
 16.1 µm/m-°C
@Temperature 25.0 - 500 °C
8.94 µin/in-°F
@Temperature 77.0 - 932 °F
 16.4 µm/m-°C
@Temperature 25.0 - 600 °C
9.11 µin/in-°F
@Temperature 77.0 - 1110 °F
 16.9 µm/m-°C
@Temperature 25.0 - 700 °C
9.39 µin/in-°F
@Temperature 77.0 - 1290 °F
 17.3 µm/m-°C
@Temperature 25.0 - 800 °C
9.61 µin/in-°F
@Temperature 77.0 - 1470 °F
 17.6 µm/m-°C
@Temperature 25.0 - 900 °C
9.78 µin/in-°F
@Temperature 77.0 - 1650 °F
 17.8 µm/m-°C
@Temperature 25.0 - 1000 °C
9.89 µin/in-°F
@Temperature 77.0 - 1830 °F
Specific Heat Capacity 0.467 J/g-°C0.112 BTU/lb-°FRT
 0.483 J/g-°C
@Temperature 100 °C
0.115 BTU/lb-°F
@Temperature 212 °F
 0.500 J/g-°C
@Temperature 200 °C
0.120 BTU/lb-°F
@Temperature 392 °F
 0.522 J/g-°C
@Temperature 300 °C
0.125 BTU/lb-°F
@Temperature 572 °F
 0.531 J/g-°C
@Temperature 400 °C
0.127 BTU/lb-°F
@Temperature 752 °F
 0.558 J/g-°C
@Temperature 500 °C
0.133 BTU/lb-°F
@Temperature 932 °F
 0.607 J/g-°C
@Temperature 600 °C
0.145 BTU/lb-°F
@Temperature 1110 °F
 0.647 J/g-°C
@Temperature 700 °C
0.155 BTU/lb-°F
@Temperature 1290 °F
 0.655 J/g-°C
@Temperature 800 °C
0.157 BTU/lb-°F
@Temperature 1470 °F
 0.660 J/g-°C
@Temperature 900 °C
0.158 BTU/lb-°F
@Temperature 1650 °F
 0.663 J/g-°C
@Temperature 1000 °C
0.158 BTU/lb-°F
@Temperature 1830 °F
 0.667 J/g-°C
@Temperature 1100 °C
0.159 BTU/lb-°F
@Temperature 2010 °F
 0.671 J/g-°C
@Temperature 1200 °C
0.160 BTU/lb-°F
@Temperature 2190 °F
Thermal Conductivity 11.4 W/m-K79.1 BTU-in/hr-ft²-°FRT
 12.6 W/m-K
@Temperature 100 °C
87.4 BTU-in/hr-ft²-°F
@Temperature 212 °F
 14.3 W/m-K
@Temperature 200 °C
99.2 BTU-in/hr-ft²-°F
@Temperature 392 °F
 15.9 W/m-K
@Temperature 300 °C
110 BTU-in/hr-ft²-°F
@Temperature 572 °F
 17.5 W/m-K
@Temperature 400 °C
121 BTU-in/hr-ft²-°F
@Temperature 752 °F
 19.0 W/m-K
@Temperature 500 °C
132 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.6 W/m-K
@Temperature 600 °C
143 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 22.2 W/m-K
@Temperature 700 °C
154 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 23.8 W/m-K
@Temperature 800 °C
165 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 25.4 W/m-K
@Temperature 900 °C
176 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 27.1 W/m-K
@Temperature 1000 °C
188 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1300 °C2370 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.10 %0.10 %
Boron, B 0.0040 %0.0040 %
Carbon, C 0.050 %0.050 %
Chromium, Cr 25 %25 %
Cobalt, Co <= 3.0 %<= 3.0 %
Iron, Fe 33 %33 %
Manganese, Mn 0.70 %0.70 %
Molybdenum, Mo <= 2.5 %<= 2.5 %
Nickel, Ni 37 %37 %
Niobium, Nb (Columbium, Cb) 0.70 %0.70 %
Nitrogen, N 0.20 %0.20 %
Silicon, Si 0.60 %0.60 %
Tungsten, W <= 2.5 %<= 2.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Rene 85 Nickel Superalloy
ATI Allvac® Rene 41® Nickel Superalloy, Heat Treatment: 1079°C (1975°F) + Age
Haynes HR-120® alloy, solution heat-treated
Haynes HR-224® Nickel Alloy
MetalTek HAYNES® HR120 Severe Corrosion and Heat Resistant Alloy

NH120A / 16310

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.