MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Braskem HB0454 HDPE Blow Molding Polyethylene Copolymer  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Blow Molding Grade

Material Notes: HB0454 is a high-density polyethylene copolymer resin with average molecular weight produced by the Unipol® process. A bottle made with HB0454 shows excellent processability, color, and superficial appearance, good chemical resistance, resistance to piling up, and does not have residual odor. Barbs can be detached easily since it has also been adjusted for use in high productivity rotating machines. Its applications include: small medicine bottles and bottles for cleaning products, cosmetics, food products, and tensioactive products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.954 g/cc0.0345 lb/in³ASTM-D792
ESCR 100% Igepal® 46 hour
@Thickness 2.00 mm,
Temperature 50.0 °C
46 hour
@Thickness 0.0787 in,
Temperature 122 °F
0.3 mm notched-plaques; ASTM-D1693
ESCR 10% Igepal® 23 hour
@Thickness 2.00 mm,
Temperature 50.0 °C
23 hour
@Thickness 0.0787 in,
Temperature 122 °F
0.3 mm notched-plaques; ASTM-D1693
Melt Flow  0.36 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.36 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM-D1238
 32 g/10 min
@Load 21.6 kg,
Temperature 190 °C
32 g/10 min
@Load 47.6 lb,
Temperature 374 °F
ASTM-D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5959ASTM-D2240
Tensile Strength at Break 31.0 MPa4500 psiASTM-D638
Tensile Strength, Yield 29.0 MPa4210 psiASTM-D638
Flexural Modulus, 1% Secant 1010 MPa146000 psiASTM-D790
Izod Impact, Notched 1.09 J/cm2.04 ft-lb/inASTM-D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 69.0 °C156 °FASTM-D648
Vicat Softening Point 127 °C
@Load 1.02 kg
261 °F
@Load 2.25 lb
ASTM-D1525

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Braskem HB0454HR HDPE Blow Molding Polyethylene Copolymer
Braskem GF4950HS HDPE Blow Molding Polyethylene Copolymer
Braskem GF5250 HDPE Blow Molding Polyethylene Copolymer
Braskem Green PE SHA7260 Injection Molding High Density Polyethylene
Braskem IG58 HDPE Injection Molding Polyethylene Copolymer

PBRAS890 / 106736

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.