MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay HTM® 552 Bismaleimide Resin
Categories: Polymer; Thermoset; Bismaleimide (BMI)

Material Notes: Description: HTM552 is a bismaleimide resin matrix formulation that combines high temperature end-use performance with good hanleability during lay-up. HTM552 has been developed for use in structures whre critical load-bearing performance is required at temperatures greater than 200°C (392°F). In applications where components may be lightly loaded, intermittent periods at 250°C (482°F) can be sustained. HTM552 is also capable of enduring very short-term exposure to a temperature of 280°C (536°F).

Features & Benefits:

  • 30 day tack life at 21°C (70°F)
  • 12 months storage at -18°C (0°F)
  • Initial cure temperature of 190°C (374°F)
  • Excellent tack and drape
  • High flow system
  • DMA E’ onset Tg of 282°C (540°F)
Note 1: Material: HTM552-FT300B40B-199g/m2-2x2 twill; Cure: 6 hrs at 190° (374°F), 6.2 bar (90 psi)
Note 2: Material: HTM552-AS4 (12K)-145g/m2-carbon fiber unitape; Cure: 6 hrs at 190° (374°F), 6.2 bar (90 psi); Post cure: 6 hrs at 240°C (464°F)

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.21 g/cc0.0437 lb/in³Cured Resin
Storage Temperature -18.0 °C-0.400 °F
 
Mechanical PropertiesMetricEnglishComments
Flexural Strength  1028 MPa
@Temperature 177 °C
149100 psi
@Temperature 351 °F
0/90°, Note 1; CRAG 200
 1029 MPa
@Temperature 24.0 °C
149200 psi
@Temperature 75.2 °F
0/90°, Note 1; CRAG 200
 1246 MPa
@Temperature 120 °C
180700 psi
@Temperature 248 °F
0/90°, Note 1; CRAG 200
Flexural Modulus  57.0 GPa
@Temperature 177 °C
8270 ksi
@Temperature 351 °F
0/90°, Note 1; CRAG 200
 68.0 GPa
@Temperature 24.0 °C
9860 ksi
@Temperature 75.2 °F
0/90°, Note 1; CRAG 200
 71.0 GPa
@Temperature 120 °C
10300 ksi
@Temperature 248 °F
0/90°, Note 1; CRAG 200
Compressive Strength 1590 MPa
@Temperature 24.0 °C
231000 psi
@Temperature 75.2 °F
0°, Note 2; ASTM D3410
Shear Strength  56.0 MPa
@Temperature 177 °C
8120 psi
@Temperature 351 °F
0/90° Interlaminar. Note 1; CRAG 100
 60.0 MPa
@Temperature 177 °C
8700 psi
@Temperature 351 °F
0° Interlaminar. Note 2, wet; CRAG 100
 83.01 MPa
@Temperature 177 °C
12040 psi
@Temperature 351 °F
0° Interlaminar. Note 2; CRAG 100
 84.1 MPa
@Temperature 120 °C
12200 psi
@Temperature 248 °F
0/90° Interlaminar. Note 1; CRAG 100
 90.3 MPa
@Temperature 24.0 °C
13100 psi
@Temperature 75.2 °F
0/90° Interlaminar. Note 1; CRAG 100
 101.0 MPa
@Temperature 24.0 °C
14650 psi
@Temperature 75.2 °F
0° In plane, Note 2; ASTM D3518
 119.0 MPa
@Temperature 24.0 °C
17260 psi
@Temperature 75.2 °F
0° Interlaminar. Note 2; CRAG 100
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 200 °C392 °Fload-bearing
 250 °C482 °Flightly loaded, intermittent
Glass Transition Temp, Tg 195 °C383 °F6 hrs at 190°C
 282 °C540 °F6 hrs at 190°C + 6 hrs at 240°C
 
Processing PropertiesMetricEnglishComments
Shelf Life 12.0 Month12.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay HTM® 556 BMI
Hexcel® HexPly® F650 Bismaleimide Resin
HOS-Technik Homide 250 Bismaleimide Resin
Hexcel® HexPly® F652 Bismaleimide Resin
Hexcel® HexPly® M65 Bismaleimide Resin

PCYTED175 / 180477

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.