MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Special Metals DURANICKEL® 301 (UNS N03301) Annealed Rod and Bar
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Tensile strength (ultimate and yield), compressive strength, hardness, and elongation values reported here are typical for Annealed Rod and Bar specifically. Other property values are typical of annealed DURANICKEL® alloy 301 or the alloy in general.

Data provided by the manufacturer, Special Metals.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.19 g/cc0.296 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 135 - 185135 - 1853000 kg
Hardness, Rockwell B 75 - 9075 - 90
Tensile Strength, Ultimate 621 - 827 MPa90000 - 120000 psi
Tensile Strength, Yield 207 - 414 MPa
@Strain 0.2 %
30000 - 60000 psi
@Strain 0.2 %
Elongation at Break 35 - 55 %35 - 55 %
Tensile Modulus 207 GPa30000 ksi
Compressive Yield Strength 362 MPa52500 psi(0.2% Offset)
Poissons Ratio 0.310.31
Shear Modulus 76.0 GPa11000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000424 ohm-cm0.0000424 ohm-cmAged
Magnetic Permeability 4.284.28Annealed Strip at 200 Oersted (15.9 kA/m)
Curie Temperature 15.0 - 50.0 °C59.0 - 122 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  13.0 µm/m-°C
@Temperature 21.0 - 100 °C
7.22 µin/in-°F
@Temperature 69.8 - 212 °F
Mean; aged
 14.0 µm/m-°C
@Temperature 21.0 - 300 °C
7.78 µin/in-°F
@Temperature 69.8 - 572 °F
Mean; aged
 14.7 µm/m-°C
@Temperature 21.0 - 500 °C
8.17 µin/in-°F
@Temperature 69.8 - 932 °F
Mean; aged
 16.6 µm/m-°C
@Temperature 21.0 - 900 °C
9.22 µin/in-°F
@Temperature 69.8 - 1650 °F
Mean; aged
Specific Heat Capacity 0.435 J/g-°C
@Temperature 20.0 - 100 °C
0.104 BTU/lb-°F
@Temperature 68.0 - 212 °F
Thermal Conductivity 23.8 W/m-K165 BTU-in/hr-ft²-°FAge Hardened
Melting Point 1400 - 1440 °C2550 - 2620 °F
Solidus 1400 °C2550 °F
Liquidus 1440 °C2620 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 4.0 - 4.75 %4.0 - 4.75 %
Carbon, C <= 0.30 %<= 0.30 %
Copper, Cu <= 0.25 %<= 0.25 %
Iron, Fe <= 0.60 %<= 0.60 %
Manganese, Mn <= 0.50 %<= 0.50 %
Nickel, Ni >= 93 %>= 93 %Including Cobalt
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.010 %<= 0.010 %
Titanium, Ti 0.25 - 1.0 %0.25 - 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals DURANICKEL® 301 (UNS N03301) Annealed and Aged Rod and Bar
321 Stainless Steel, annealed and cold drawn bar, 25 mm diam.
Alclad Aluminum 7075-T6, T651
Special Metals DURANICKEL® 301 (UNS N03301) Cold-Drawn Rod and Bar
Special Metals INCONEL® 625LCF® Nickel Superalloy (UNS N06626) Annealed + 20% Cold Work

NINCO66 / 17500

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.