MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sumitomo Bakelite Sumikon® PM-6630 Type Black Phenolic Novolac
Categories: Polymer; Thermoset; Phenolic; Phenolic, Novolac, Mineral/Glass Filled

Material Notes: SUMIKON PM-6630 Type Black is a short glass fiber & mineral molding compound based on a phenolic novolac polymer. It is supplied in the form of granular/molding powder for molding. This grade is officially registered UL with V-0 (t=3.0).

Information provided by Sumitomo Bakelite High Performance Plastics (sbhpp)

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.78 g/cc1.78 g/ccJIS K 6911
Linear Mold Shrinkage 0.0018 cm/cm0.0018 in/inJIS K 6911
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 122 MPa17700 psiJIS K 6911
Flexural Strength 228 MPa33100 psiJIS K 6911
Flexural Modulus 18.3 GPa2650 ksiJIS K 6911
Charpy Impact, Notched 0.470 J/cm²2.24 ft-lb/in²JIS K 6911
 
Electrical PropertiesMetricEnglishComments
Insulation Resistance 5.00e+11 ohm5.00e+11 ohmAfter boiling; JIS K 6911
 3.00e+12 ohm3.00e+12 ohmAs mold; JIS K 6911
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 231 °C448 °FJIS K 6911
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Sumitomo Bakelite Sumikon® PM-9610 Phenolic, Compression Grade
Sumitomo Bakelite Sumikon® PM-6830 Type Black Phenolic Resol
Sumitomo Bakelite Sumikon® PM-9501 Type J Black Phenolic Novolac

PSUMIT456 / 194261

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.